High-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material and preparation method thereof

By introducing spherical equiatomic ratio TiZrNbV high-entropy alloy particles into copper-based materials, and using ball milling and vacuum hot-pressing sintering processes, high-strength and high-toughness TiZrNbV high-entropy alloy particle-reinforced copper-based composite materials are formed, solving the problems faced by traditional ceramics and carbon materials. The interface bonding problem in the copper matrix achieves high strength, high toughness and excellent conductive properties of copper-based materials, which are suitable for aerospace, automobile and rail transit fields.

CN118814014APending Publication Date: 2024-10-22JINAN UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410810153.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The conductivity and plasticity of traditional ceramic particle-reinforced copper-based materials are poor. The dispersion and interface bonding problems of carbon materials in the copper matrix reduce the reinforcement efficiency, making it difficult to simultaneously improve the mechanical properties and electrical and thermal conductivity of copper-based materials.

Method used

Spherical equiatomic ratio TiZrNbV high-entropy alloy particles are used as reinforcements. Through ball milling, cleaning, and vacuum hot-pressing sintering processes, high-strength and high-toughness TiZrNbV high-entropy alloy particle-reinforced copper-based composite materials are formed to achieve the integration of copper matrix and high-entropy alloy particles. The metallurgical interface bonding between them overcomes the interface bonding weaknesses of traditional ceramic particles and carbon materials.

Benefits of technology

It achieves high strength, high toughness and excellent electrical conductivity of copper-based composite materials, resolves the contradiction between mechanical properties and electrical properties, and has broad application prospects, especially in the fields of aerospace, automobiles and rail transit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118814014A_ABST
    Figure CN118814014A_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material and a preparation method thereof.The preparation method comprises the steps that spherical equal-atomic-ratio TiZrNbV high-entropy alloy particles are subjected to ball milling, a process control agent is added in the ball milling process, and shielding gas is introduced to prevent oxidation; the TiZrNbV high-entropy alloy particles obtained after ball milling are cleaned so as to remove the process control agent, and then vacuum drying is conducted; mixing the dried TiZrNbV high-entropy alloy particles and dendritic copper powder on a ball mill to obtain composite powder; the composite powder is added into a graphite mold, and pressure is applied to the composite powder at the room temperature and kept for the preset time; a current-driven rapid sintering furnace is adopted for sintering the composite powder, and a high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material block is obtained; during sintering, an axial pressure is applied to the sample to accelerate the densification process. The contradiction between the mechanical property and the electric heat conduction property of the copper-based composite material is solved, and the requirements for light weight and high reinforcement of the material can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal matrix composite materials, and in particular to a high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper matrix composite material, and a preparation method and application thereof. Background Art

[0002] Advanced copper alloys represented by high-strength and high-conductivity copper-based composite materials not only have excellent electrical conductivity and can effectively reduce energy loss during power transmission, but also have ultra-high strength and certain toughness to serve in special and extreme environments. They can be used as some special conductive and wear-resistant parts in the fields of aerospace, automobiles, and rail transportation. The use of a composite strategy for material design can maintain the inherent high conductivity of the copper matrix while improving the material strength. This is an effective technical approach to solving the current shortcoming of low strength of copper alloys.

[0003] The addition of traditional hard ceramic particles to the copper matrix can effectively improve the mechanical properties of copper materials. However, due to the poor electrical and thermal conductivity of the ceramic particles themselves and the large difference in thermal expansion coefficient with the copper matrix, as well as the poor wettability of the ceramic particles at the copper matrix interface and the lack of interfacial reaction activity, the conductivity and plasticity of the ceramic particles reinforced copper composites are poor. In recent years, new carbon materials developed, including carbon fibers, carbon nanotubes and graphene, have structural diversity and unique properties. Introducing them into copper materials as reinforcements can improve their mechanical properties and electrical and thermal conductivity. However, the dispersion of carbon materials in the copper matrix and the interface bonding between the carbon materials and the matrix will reduce the reinforcement efficiency of the carbon materials. Summary of the invention

[0004] In order to solve the deficiencies of the above-mentioned prior art, the present invention provides a high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material and a preparation method and application thereof. By introducing TiZrNbV high-entropy alloy particle reinforcement into the copper matrix, the interface between the reinforcement and the copper matrix is ​​firmly connected. By optimizing the content of high-entropy alloy particles, the grain size of the copper matrix in the composite material is gradually refined, and the mechanical properties show an increasing trend, which can simultaneously improve the contradiction between electrical properties and mechanical properties.

[0005] The first object of the present invention is to provide a method for preparing a high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material.

[0006] The second object of the present invention is to provide a high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material.

[0007] The third object of the present invention is to provide an application of a high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material.

[0008] The first object of the present invention can be achieved by adopting the following technical solutions:

[0009] A method for preparing a high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material, the method comprising:

[0010] Spherical equal atomic ratio TiZrNbV high entropy alloy particles are ball milled, a process control agent is added during the ball milling process to reduce cold welding during the ball milling process, and a protective gas is introduced to prevent oxidation;

[0011] The ball-milled TiZrNbV high entropy alloy particles are cleaned to remove the process control agent and then vacuum dried;

[0012] The dried TiZrNbV high entropy alloy particles and the dendritic copper powder are mixed in a ball mill to obtain a composite powder;

[0013] Adding the composite powder into a graphite mold, applying pressure to the composite powder at room temperature and maintaining it for a preset time to complete pre-pressing;

[0014] The composite powder was sintered in an electric current-driven rapid sintering furnace to obtain a high-strength and high-toughness TiZrNbV high-entropy alloy particle-reinforced copper-based composite material block; during the sintering process, axial pressure was applied to the sample to accelerate the densification process.

[0015] Furthermore, the spherical equiatomic ratio TiZrNbV high entropy alloy particles have a particle size range of 10 to 90 μm and an average particle size of about 40.4 μm, and are obtained by the following method:

[0016] Ti metal block, Zr metal block, Nb metal block and V metal block are prepared by rotating electrode method after being homogenized by repeated arc melting for at least 6 times; wherein the purity of Ti metal block, Zr metal block, Nb metal block and V metal block is higher than 99.99%.

[0017] Furthermore, the spherical equiatomic ratio TiZrNbV high entropy alloy particles were ball-milled, wherein the mass ratio of the spherical equiatomic ratio TiZrNbV high entropy alloy particles to the stainless steel grinding balls was 1:10; the sizes of the stainless steel grinding balls were 10 mm: 8 mm: 5 mm, respectively, and the corresponding mass ratios were 5:3:2, respectively.

[0018] Furthermore, the protective gas is argon.

[0019] Furthermore, the ball-milled TiZrNbV high entropy alloy particles are alternately cleaned with alcohol and deionized water, wherein the alcohol concentration is 75%, and the number of alternate cleanings is not less than 5 times.

[0020] Furthermore, the dried TiZrNbV high entropy alloy particles and dendritic copper powder were mixed in a mass ratio of 1:99 to 1:4, and the mixing parameters were: a rotation speed of 300 R / min and a ball milling time of 1 h.

[0021] Furthermore, the mass of the composite powder is 120 g; the diameter of the graphite mold is 40 mm; the applied pressure is 10 MPa, and the preset time is 5 minutes.

[0022] Furthermore, the sintering process parameters are: vacuum degree is less than 10 -3 Pa, the sintering temperature is 800℃ and kept at this temperature for 30 minutes; and the axial pressure is 40MPa.

[0023] The second object of the present invention can be achieved by adopting the following technical solutions:

[0024] A high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material is prepared based on the above preparation method.

[0025] The third object of the present invention can be achieved by adopting the following technical solutions:

[0026] The invention discloses an application of a high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material, and an application of the high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material prepared by the above-mentioned preparation method in the fields of aerospace, automobile and rail transportation technology.

[0027] The present invention has the following beneficial effects compared with the prior art:

[0028] 1. The present invention adopts spherical TiZrNbV high entropy alloy particles with equal atomic ratio and dendritic copper powder as raw materials, and prepares TiZrNbV particle-reinforced copper-based composite materials through vacuum hot pressing sintering process. By combining load transfer strengthening, fine grain strengthening effect and dislocation strengthening mechanism, the limitation of single strengthening means is broken through, and the metallurgical interface bonding between the copper matrix and the TiZrNbV high entropy alloy particles is better achieved, and the interface wettability problem between the reinforcement and the copper matrix is ​​solved. While improving the strength of the copper-based composite material, high electrical conductivity and ductility are maintained. The finally obtained copper-based composite material exhibits good mechanical and electrical properties and has broad application prospects;

[0029] 2. The equiatomic ratio TiZrNbV high entropy alloy particles used in the present invention have excellent properties such as high strength, high hardness, low density, excellent high temperature stability, good plasticity and wear resistance. As a reinforcement for copper-based composite materials, a metal-metal metallurgical bonding interface can be formed between the copper matrix, overcoming the disadvantage of weak interface bonding with traditional ceramic particle reinforcements. In addition, another advantage of using TiZrNbV high entropy alloy as a reinforcement for copper-based composite materials is that the solid solubility of elements such as Ti, Zr, Nb, and V in copper is relatively low at room temperature, which has little effect on its electrical conductivity. Therefore, the use of TiZrNbV high entropy alloy reinforcements can avoid the influence of solid solution and microstructure evolution on the electrical and mechanical properties of composite materials under high temperature conditions, thereby preparing high-strength and high-conductivity copper-based composite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0031] Figure 1 The microscopic morphology and XRD spectrum of the raw material powder used in the present invention; wherein, (a) is the microscopic morphology of dendritic copper powder, (b) is the XRD spectrum of dendritic copper powder, (c) is the microscopic morphology of TiZrNbV particles after ball milling, and (d) is the XRD spectrum of TiZrNbV particles after ball milling;

[0032] Figure 2 The microstructure and element distribution diagram of TiZrNbV / Cu composite materials; (a) 5wt.% composite material and enlarged illustration, (b) 15wt.% composite material, (c) element distribution diagram of the selected area of ​​15wt.% composite material;

[0033] Figure 3 (a1) to (e1) correspond to the metallographic phase diagrams and grain size distribution diagrams of the TiZrNbV / Cu composite materials of Examples 1 to 5, respectively;

[0034] Figure 4 The hardness, conductivity and density distribution bar graphs of the comparative example and Examples 1 to 5 are shown in FIG.

[0035] Figure 5 The hardness, conductivity and density distribution bar graphs of the comparative example and Examples 5 to 8 are shown in FIG.

[0036] Figure 6 The stress-strain curves of the TiZrNbV / Cu composite materials of Examples 1 to 5 and the pure copper of the comparative example;

[0037] Figure 7 It is the distribution diagram of yield strength, tensile strength and elongation of comparative example and Examples 1 to 5;

[0038] Figure 8 It is a distribution diagram of the yield strength, tensile strength and elongation of the comparative example and Examples 5 to 8. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. It should be understood that the specific embodiments described are only used to explain the present application and are not used to limit the present application.

[0040] The density of the TiZrNbV high entropy alloy particle reinforced copper-based composite material in the embodiment is measured by a high-precision density meter (MI-120). To ensure the accuracy of the data, the sample is cleaned with alcohol before testing to prevent bubbles from existing on the sample during the test. Each sample is measured 3 times and the arithmetic average is taken.

[0041] The electrical conductivity of the TiZrNbV high entropy alloy particle reinforced copper-based composite material in the embodiment is measured by an eddy current digital conductivity meter (PZ60A). To ensure the reliability of the conductivity results, the sample surface is polished with sandpaper before testing, and the sample surface is measured five times after cleaning with alcohol, and the arithmetic mean is taken as the conductivity of the sample.

[0042] The microhardness of the TiZrNbV high entropy alloy particle reinforced copper-based composite material in the embodiment is tested by a HXD-1000TMSC / LCD digital Vickers microhardness tester, the unit is HV, the applied load is 100 grams, and the probe is held for 15 seconds after being pressed in. To ensure the accuracy of the data, 10 points are taken on the sample surface for testing, and the arithmetic mean is taken as the microhardness of the sample.

[0043] The tensile properties of the TiZrNbV high entropy alloy particle reinforced copper-based composite material in the embodiment are tested on a MTSE45 universal testing machine. The tensile specimen is a 5×2 mm 2, non-standard tensile specimens with a gauge length of 10 mm, and a loading rate of 0.5 mm / min. At the same time, to ensure the reliability and reproducibility of the data, the surface of the tensile sample was polished flat with sandpaper before the tensile test to avoid stress concentration during the test that would affect the experimental results. Three tensile specimens were taken for each mass fraction of the composite material for testing.

[0044] Embodiment 1:

[0045] A high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material is prepared by the following steps:

[0046] (1) Ball milling: Weigh 50g of spherical equiatomic TiZrNbV high entropy alloy particles and 500g of stainless steel grinding balls and put them into a planetary ball mill for ball milling. The microstructure of the TiZrNbV high entropy alloy particles is composed of a body-centered cubic (BCC) phase and a small amount of V2Zr phase. Nb and V are BCC structure stabilizing elements. Due to the solid solution strengthening effect and low valence electron concentration, TiZrNbV exhibits relatively high strength and plasticity, and has the characteristics of low density and high specific yield strength. The size ratio of the stainless steel ball is: 10mm: 8mm: 5m, and the mass ratio of the corresponding size is 5:3:2. 5ml of n-heptane is added as a process control agent to reduce cold welding during ball milling, and argon is introduced as a protective gas. The ball milling parameters are a rotation speed of 400R / min and a ball milling time of 4h. The surface of the obtained TiZrNbV high entropy alloy particles is relatively rough, and the powder shape mainly includes irregular spheres and flakes, such as Figure 1 (c) as shown.

[0047] (2) Cleaning and drying: The ball-milled TiZrNbV particles were cleaned five times with 75% alcohol and deionized water alternately to remove n-heptane, and then dried in a vacuum drying oven at 60°C. Figure 1 (d) is the XRD spectrum of the TiZrNbV high entropy alloy particles after drying. It can be seen that the powder is relatively pure and only has BCC structure.

[0048] (3) Mixing: Weigh 1.2 g TiZrNbV high entropy alloy particles and 118.8 g dendritic copper powder, without adding grinding balls, and mix them in a ball mill at a speed of 300 R / min for 1 h to obtain a composite powder. The shape of the dendritic copper powder is shown in Figure 2. Figure 1 (a), XRD spectrum reference Figure 1 (b).

[0049] (4) Cold pressing: 120 g of the composite powder was added into a graphite mold with a diameter of 40 mm, and a pressure of 4 MPa was applied to it at room temperature for 5 min for pre-pressing.

[0050] (5) Vacuum hot pressing sintering: Using current driven fast sintering furnace (FHP-828), the vacuum degree is less than 10 -3 Pa, the sintering temperature was kept at 800°C for 30 min, and the composite powder was sintered to obtain a 1wt.% TiZrNbV / Cu composite material. During the sintering process, an axial pressure of 40 MPa was applied to the sample to accelerate the densification process, and a sample with a diameter of about 40 mm and a height of 10 mm was obtained.

[0051] Embodiment 2:

[0052] On the basis of Example 1, the difference of this example is that the content of TiZrNbV high entropy alloy particles is different, namely 2.4g TiZrNbV high entropy alloy particles and 117.6g dendritic copper powder, and the rest is the same as Example 1.

[0053] Embodiment 3:

[0054] On the basis of Example 1, the difference of this example is that the content of TiZrNbV high entropy alloy particles is different, namely 3.6 g TiZrNbV high entropy alloy particles and 116.4 g dendritic copper powder, and the rest is the same as Example 1.

[0055] Embodiment 4:

[0056] Based on Example 1, the difference of this example is that the content of TiZrNbV high entropy alloy particles is different, namely 4.8 g TiZrNbV high entropy alloy particles and 115.2 g dendritic copper powder, and the rest is the same as Example 1.

[0057] Embodiment 5:

[0058] On the basis of Example 1, the difference of this example is that the content of TiZrNbV high entropy alloy particles is different, namely 6.0 g TiZrNbV high entropy alloy particles and 114.0 g dendritic copper powder, and the rest is the same as Example 1.

[0059] Embodiment 6:

[0060] On the basis of Example 1, the difference of this example is that the content of TiZrNbV high entropy alloy particles is different, namely, 12.0 g TiZrNbV high entropy alloy particles and 108.0 g dendritic copper powder, and the rest is the same as Example 1.

[0061] Embodiment 7:

[0062] On the basis of Example 1, the difference of this example is that the content of TiZrNbV high entropy alloy particles is different, namely, 18.0 g TiZrNbV high entropy alloy particles and 102.0 g dendritic copper powder, and the rest is the same as Example 1.

[0063] Embodiment 8:

[0064] On the basis of Example 1, the difference of this example is that the content of TiZrNbV high entropy alloy particles is different, namely, 24.0 g TiZrNbV high entropy alloy particles and 96.0 g dendritic copper powder, and the rest is the same as Example 1.

[0065] Comparative Example:

[0066] 120 g of dendritic copper powder was weighed and sintered using the same sintering process parameters as in Example 1 to obtain a pure copper comparison sample.

[0067] The microscopic morphology and element distribution diagrams of the TiZrNbV / Cu composite materials with different mass fractions in the above-mentioned Examples 5 and 7 are shown in FIG. Figure 2 As shown. The dark part in the figure is the copper matrix, and the light particles are the TiZrNbV high entropy alloy reinforcements. It can be seen from the figure that there are no obvious microscopic defects such as holes and cracks in the microstructure of the composite material, indicating that the TiZrNbV / Cu composite material sintered at a temperature of 800°C has good compactness, and the density and compactness corresponding to the sample are shown in Table 1. At the same time, it was observed that the reinforcement phase of Example 5 was distributed more evenly in the copper matrix, while a small amount of agglomeration of the reinforcement phase was found in the composite material with a content of Example 7. At the same time, it can be seen that a "core-shell" structure appears in the reinforcement, and the matrix and the reinforcement diffuse with each other to form a metal transition layer, forming a good metallurgical bonding interface with the matrix, indicating that the TiZrNbV / Cu interface is firmly connected. In order to better analyze the distribution law of each element in the "core-shell" structure, the Figure 2 (a) Element analysis was performed at the positions corresponding to the numbers in the illustration. As shown in Table 2, copper was detected on the diffusion layer on the TiZrNbV HEA side, and the percentage of copper atoms decreased with the distance from the center of the reinforcement, indicating that obvious interface diffusion reaction occurred between TiZrNbV HEA and copper matrix during the sintering process.

[0068] Table 1 Atomic percentage of each element in the composite material (at.%)

[0069]

[0070] Figure 3The surface morphology of the TiZrNbV / Cu composite materials with different mass fractions in Examples 1 to 5 after etching can be seen from the size distribution diagram of the composite materials that the matrix grain size of the composite materials with different mass fractions is mainly concentrated between 2 and 4 μm, and as the mass fraction of TiZrNbV particles increases, the grain refinement phenomenon becomes more obvious. The matrix grain size of the prepared composite materials changes from mainly concentrated in 2 to 6 μm (Examples 1 and 2) to mainly concentrated in 0 to 4 μm (Examples 3 to 5), showing a significant grain refinement effect, which can be attributed to the synergistic effect of multiple micro-strengthening mechanisms. First, the uniform dispersion of TiZrNbV particles provides grain boundary dispersion strengthening, effectively limits the grain boundary migration rate, and inhibits grain growth; secondly, HEA particles, as heterogeneous nucleation sites, reduce the nucleation energy barrier, promote the formation of new grains in the copper-based composite material, and refine the grain size; finally, the solid solution of some high entropy alloy elements may also affect the grain boundary migration, further refining the grains.

[0071] Figure 4 The hardness, conductivity and density of the samples of Examples 1 to 5 and the comparative examples are shown in Table 2. The hardness of the samples of the examples is significantly higher than that of the unreinforced comparative examples, and it increases with the increase of the mass fraction of the reinforcing phase. The hardness of Example 1 is 88±2.1HV0.1, which is about 49% higher than that of the comparative example (59±2.3HV0.1). The hardness of Example 5 is as high as 109±5.5HV0.1, which is about 84% higher than that of the unreinforced matrix. On the contrary, the conductivity of the five composite materials decreases with the increase of the content, but the decreasing trend is much lower than the increasing trend of the hardness. The conductivity of Example 5 (77.7±0.41%IACS) is only about 21% lower than that of the comparative example (98.3±0.44%IACS). The higher density (see Table 1) is one of the reasons why the mechanical properties of the copper-based composite material are greatly improved while maintaining higher electrical properties as much as possible, and it also shows the effectiveness and suitability of the sintering process parameters. In addition, the grain refinement caused by the introduction of TiZrNbV high entropy alloy particles (see Figure 3 ), which further promotes the improvement of hardness through the Hall-Petch effect.

[0072] Figure 5It is a comparative distribution diagram of some mechanical properties of comparative examples and embodiments 5 to 8. It can be seen from the figure that when the mass proportion of TiZrNbV high entropy alloy increases from 5wt.% to 20wt.%, the density of the composite material gradually decreases. This is mainly attributed to the fact that under normal circumstances, the increase in the content of TiZrNbV reinforcing phase particles in copper-based composite materials is often accompanied by an increase in the number of pores, resulting in a decrease in the relative density of the material; at the same time, because hard particles will limit the migration and elimination of pores, the increase in the content of reinforcing phase particles will weaken the sintering ability of the material, and the particle agglomeration phenomenon will also promote the formation of pores. Therefore, as the content of the reinforcement increases, the increase in the porosity of the material will reduce its density. It can also be seen from the figure that the hardness of the composite material has been significantly improved. The hardness of Example 8 reached 117.3±6.08HV0.1, which is nearly 106% higher than that of pure copper. However, the conductivity of the high-content composite material also suffered a large loss. The conductivity of Example 8 was only 18.7±0.08%IACS, which is closely related to its high mass fraction of the second phase and relatively low density.

[0073] Table 2 Microhardness, conductivity, density and compactness of Examples 1 to 8 and Comparative Examples

[0074]

[0075]

[0076] The stress-strain curves of the tensile tests carried out at room temperature for the comparative examples and embodiments 1 to 5 are as follows: Figure 6 The distribution diagrams of yield strength, tensile strength and elongation are shown in Figure 7As shown, the specific values ​​are shown in Table 3. The strength of Examples 1 to 5 is significantly higher than that of the comparative example, and the strength continues to increase with the increase of mass fraction. This is attributed to the dual hindering effect of grain refinement and the addition of reinforcement particles on dislocation movement. Grain refinement increases the grain boundary density, thereby providing more obstacles for dislocation movement, and TiZrNbV particles further hinder the slip of dislocations, which together promote the improvement of the strength of the composite material. The yield strength of Example 5 is as high as 212±6.8MPa and the tensile strength reaches 305±8.6MPa, which are about 108% and 45% higher than the comparative example, respectively. In terms of elongation, as the content of TiZrNbV particles increases, its plasticity is observed to gradually decrease. The fracture strains containing Example 1 and Example 5 reached 35.6±1.18% and 25.2±1.59%, respectively, which are slightly lower than the comparative example (38.1±1.33%) without TiZrNbV particles. This can be attributed to the fact that the higher mass fraction of hard reinforcement particles leads to more microscopic defects and increased stress concentration during plastic deformation. These hard particles act as non-matching deformation areas during material deformation, and dislocations can continue to multiply in pure copper grains. However, cracks and interface debonding begin to gradually appear in the composite material, increasing the inhomogeneity of local stress and thus reducing the overall plasticity of the material.

[0077] Table 3 Tensile properties of Examples 1 to 8 and Comparative Examples

[0078]

[0079] The tensile properties of the comparative examples and examples 5 to 8 include the distribution diagrams of yield strength, tensile strength and elongation. Figure 8 As shown, the specific values ​​are shown in Table 3. It can be seen that with the increase in the mass fraction of TiZrNbV reinforcement material, the strength of the TiZrNbV / Cu composite material is significantly improved. Specifically, the yield strength and tensile strength of Example 8 reach 272.7±11.18MPa and 357.7±9.30MPa, respectively. However, it is worth noting that the strain rate of the composite material shows a trend opposite to the strength, and its strain rate is only 8.79±1.06%.

[0080] Through the microstructural analysis of TiZrNbV / Cu composite materials, it is found that the TiZrNbV / Cu interface is firmly connected, and a "core-shell" structure appears in the reinforcement due to element diffusion, indicating that a good metallurgical bonding interface is formed with the copper matrix, and the elements of the matrix and the reinforcement diffuse significantly at the "shell", accompanied by the formation of intermetallic compounds. With the increase of the mass fraction of TiZrNbV high entropy alloy particles, the grain size of the composite matrix gradually refines. With the increase of the mass fraction of TiZrNbV, the mechanical properties of TiZrNbV / Cu composite materials show an increasing trend. Through the performance analysis of TiZrNbV / Cu composite materials with different contents, it is found that Example 5 has a highly dense structure, its conductivity is 77.7%IACS, its microhardness is 109HV0.1, its yield strength, tensile strength and elongation are 212MPa, 305MPa and 25.2% respectively, achieving a good balance between electrical properties and mechanical properties.

[0081] In summary, the present invention ball-mills, cleans and dries high entropy alloy particles, then mixes the high entropy alloy particles and copper powder in different mass ratios, and then obtains a high entropy alloy particle-reinforced copper bulk composite material by vacuum rapid sintering technology. The composite materials all have a high-density structure, the reinforcement particles are evenly distributed in the copper matrix and the interface of the two is well bonded, and the high entropy alloy reinforcement particles can reduce the grain size in the copper matrix of the composite material, achieve high strength, high toughness and excellent electrical conductivity. The present invention not only solves the contradiction between the mechanical properties and electrical and thermal conductivity of copper-based composite materials, but also can meet the requirements of lightweight and high strengthening of materials.

[0082] The above is only a preferred embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solution and inventive concept of the present invention within the scope disclosed by the present invention, which shall fall within the protection scope of the present invention.

Claims

1. A method for preparing a high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material, characterized in that: The method comprises: Spherical equal atomic ratio TiZrNbV high entropy alloy particles are ball milled, a process control agent is added during the ball milling process to reduce cold welding during the ball milling process, and a protective gas is introduced to prevent oxidation; The ball-milled TiZrNbV high entropy alloy particles are cleaned to remove the process control agent and then vacuum dried; The dried TiZrNbV high entropy alloy particles and the dendritic copper powder are mixed in a ball mill to obtain a composite powder; Adding the composite powder into a graphite mold, applying pressure to the composite powder at room temperature and maintaining it for a preset time to complete pre-pressing; The composite powder was sintered in an electric current-driven rapid sintering furnace to obtain a high-strength and high-toughness TiZrNbV high-entropy alloy particle-reinforced copper-based composite material block; during the sintering process, axial pressure was applied to the sample to accelerate the densification process.

2. The preparation method according to claim 1, characterized in that: The spherical equiatomic ratio TiZrNbV high entropy alloy particles have a particle size range of 10 to 90 μm and an average particle size of about 40.4 μm, and are obtained by the following method: Ti metal block, Zr metal block, Nb metal block and V metal block are prepared by rotating electrode method after being homogenized by repeated arc melting for at least 6 times; wherein the purity of Ti metal block, Zr metal block, Nb metal block and V metal block is higher than 99.99%.

3. The preparation method according to claim 1, characterized in that: Spherical equiatomic ratio TiZrNbV high entropy alloy particles are ball-milled, wherein the mass ratio of the spherical equiatomic ratio TiZrNbV high entropy alloy particles to stainless steel grinding balls is 1:10; the sizes of the stainless steel grinding balls are 10 mm: 8 mm: 5 mm, respectively, and the corresponding mass ratios are 5:3:2, respectively.

4. The preparation method according to claim 1, characterized in that: The protective gas is argon.

5. The preparation method according to claim 1, characterized in that: The ball-milled TiZrNbV high entropy alloy particles are cleaned alternately with alcohol and deionized water, wherein the alcohol concentration is 75%, and the number of alternate cleanings is not less than 5 times.

6. The preparation method according to claim 1, characterized in that: The dried TiZrNbV high entropy alloy particles and dendritic copper powder are mixed in a mass ratio of 1:99 to 1:4, and the mixing parameters are: rotation speed of 300R / min, and ball milling time of 1h.

7. The preparation method according to claim 1, characterized in that: The mass of the composite powder is 120 g; the diameter of the graphite mold is 40 mm; the applied pressure is 10 MPa, and the preset time is 5 minutes.

8. The preparation method according to claim 1, characterized in that: Sintering process parameters: vacuum degree less than 10 -3 Pa, the sintering temperature is 800℃ and kept at this temperature for 30 minutes; and the axial pressure is 40MPa.

9. A high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material, characterized in that: It is prepared based on the preparation method according to any one of claims 1 to 8.

10. An application of a high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite material, characterized in that: Application of high-strength and high-toughness TiZrNbV high-entropy alloy particle reinforced copper-based composite materials prepared by the preparation method according to any one of claims 1 to 8 in the fields of aerospace, automobile, and rail transportation technology.