Iridium-containing catalyst as well as preparation method and application thereof

By using TiO2-coated TiN carrier to support elemental iridium, the problem of high dosage of precious metals and poor activity of the anode catalyst is solved, and an efficient and low-cost hydrogen production technology by electrolyzing water is realized.

CN118814218APending Publication Date: 2024-10-22CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310423936.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In the existing proton exchange membrane electrolysis water electrolysis hydrogen production technology, the amount of precious metal used in the anode catalyst is too high and the activity is poor, resulting in high cost and low efficiency, which hinders the commercial application of the equipment.

Method used

TiO2-coated TiN is used as a carrier to load elemental iridium. By adjusting the specific surface area and conductivity of the carrier, the activity and cycle stability of the catalyst are improved, and the usage of iridium element is reduced.

Benefits of technology

It is possible to improve the catalytic activity, cycle stability and conductivity of the catalyst while maintaining a low iridium content, reduce the overpotential of the anode, and improve the efficiency of hydrogen production by electrolysis of water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118814218A_ABST
    Figure CN118814218A_ABST
Patent Text Reader

Abstract

The invention relates to an iridium-containing catalyst as well as a preparation method and application thereof. The iridium-containing catalyst comprises a carrier and an active component loaded on the carrier, the carrier comprises TiN coated with TiO2, and the active component comprises elementary substance Ir. When the catalyst is used for a proton exchange membrane water electrolysis reaction, the catalyst has relatively good catalytic activity, cycling stability and conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of hydrogen energy and electrocatalysis technology, and in particular, to an iridium-containing catalyst and a preparation method and application thereof. Background Art

[0002] With the proposal of the carbon neutrality and carbon peak targets, green hydrogen production technology has received widespread attention. Among them, the proton exchange membrane (PEM) water electrolysis hydrogen production has high operating current density, small footprint, high efficiency, and the advantages of fast start and stop and a large load adjustable range. It is very suitable for the use of renewable energy power such as photovoltaics and wind power. At present, the main problem of PEM water electrolysis hydrogen production is the high cost. It is very important to reduce the cost of the fuel cell and improve the efficiency of the catalyst through the optimization design of the catalyst.

[0003] At present, the cathode catalysts use Pt / C and Ir metal catalysts respectively. The loading amount of Pt cathode catalyst can be as low as 0.3-0.025 mg / cm 2 , within this range, the performance of hydrogen production by water electrolysis is almost not affected. In the process of PEM water electrolysis, the anode is the rate-controlling step, its overpotential is high, the amount of catalyst used is 5-10 times more than the cathode catalyst, and the price of Ir-based metals is more expensive than that of Pt-based metals. Therefore, reducing the overpotential of the oxygen evolution reaction and reducing the amount of noble metals used in the anode are important breakthroughs in achieving large-scale commercialization of PEM water electrolysis equipment.

[0004] Introducing appropriate carriers to prepare supported catalysts can effectively reduce the amount of precious metals and improve the activity of the catalyst. Many carrier materials have been reported to be used in the oxygen evolution reaction in acidic water electrolysis, such as SnO2, ATO, TiO2, Nb-TiO2, etc. Among them, TiO2 with a large specific surface area is used as a carrier of IrO2 (201811295042.7; ACS Catal. 2017, 7, 2346-2352), but the membrane electrode with low IrO2 loading has poor activity. In order to further reduce the content of precious metal iridium in the water electrolysis membrane electrode, it is necessary to further improve the conductivity of TiO2 while maintaining the acid and oxidation resistance of the TiO2 carrier. Summary of the invention

[0005] The purpose of the present disclosure is to provide an iridium-containing catalyst and a preparation method and application thereof. When the catalyst is used in a proton exchange membrane water electrolysis reaction, it has good catalytic activity, cycle stability and conductivity.

[0006] In order to achieve the above-mentioned object, the present disclosure provides, in a first aspect, an iridium-containing catalyst, the iridium-containing catalyst comprising a carrier and an active component supported on the carrier;

[0007] The carrier includes TiN coated with TiO2, and the active component includes single substance Ir.

[0008] Optionally, the specific surface area of ​​the iridium-containing catalyst is 40-70 m 2 / g;

[0009] The average particle size of the active component is 2-4 nm;

[0010] Optionally, the conductivity of the iridium-containing catalyst is 0.005-0.03 S / mm.

[0011] Optionally, the content of the active component calculated as iridium element is 30-50 wt % relative to the total weight of the iridium-containing catalyst.

[0012] The second aspect of the present disclosure provides a carrier for anode catalyst for water electrolysis, wherein the carrier is TiN coated with TiO2, and the specific surface area of ​​the carrier is 100-150m 2 / g.

[0013] Optionally, relative to the total weight of the TiO2-coated TiN, the content of the TiO2 is 40-60 wt %, and the content of the TiN is 40-60 wt %;

[0014] The TiN is a face-centered cubic crystal;

[0015] The conductivity of the carrier is 1×10 -7 to 1.5×10 -6 S / mm.

[0016] Optionally, in the XRD spectrum of the TiO2-coated TiN, there is no characteristic peak of TiO2, and the position of the characteristic peak of TiN is shifted toward a high angle by 0.2-0.3 eV relative to the characteristic peak of pure TiN.

[0017] A third aspect of the present disclosure provides a method for preparing TiO2-coated TiN, the method comprising the following steps:

[0018] S1, mixing a complexing agent, a titanium source, TiN and water, adjusting the pH value of the mixture to 8-10 and performing a hydrolysis reaction to obtain a first material;

[0019] S2, subjecting the solid in the first material to a first heat treatment;

[0020] The complexing agent includes an organic polyacid.

[0021] Optionally, the complexing agent includes one or more organic polyacids having 2 to 10 carbon atoms, preferably one or more of ethylenediaminetetraacetic acid, oxalic acid, maleic acid and citric acid;

[0022] The titanium source includes one or more of titanium sulfate, ethyl titanate and tetrabutyl titanate;

[0023] Optionally, the particle size of the TiN is 10-20 nm.

[0024] Optionally, in step S1, the conditions of the hydrolysis reaction include: time of 3-10h, temperature of 60-100°C;

[0025] The mixing conditions include: time of 0.5-2h, temperature of 60-100°C;

[0026] The molar ratio of the titanium source, the TiN and the complexing agent calculated on the basis of titanium element is 1:(0.5-1.2):(0.5-2);

[0027] In the mixture, the concentration of the titanium source calculated as titanium element is 0.1-1 mol / L.

[0028] Optionally, in step S2, the heat treatment method is roasting, and the roasting conditions include: time of 2-8h, temperature of 300-600°C, heating rate of 2-5°C / min, and roasting atmosphere including air atmosphere with an oxygen content of 20-25% by volume.

[0029] A fourth aspect of the present disclosure provides TiO2-coated TiN prepared by the method described in the third aspect of the present disclosure.

[0030] A fifth aspect of the present disclosure provides a method for preparing an iridium-containing catalyst, the method comprising: contacting the TiO2-coated TiN, a surfactant, and an iridium source according to the second aspect or the fourth aspect of the present disclosure with an organic solvent to react;

[0031] The organic solvent includes one or more of saturated polyols, aromatic alcohols and amides.

[0032] Optionally, the surfactant comprises an organic ammonium salt having 12 to 19 carbon atoms, preferably comprising one or more of cetyltrimethylammonium chloride, tetradecyltrimethylammonium bromide and cetyltrimethylammonium bromide;

[0033] The iridium source includes chloroiridic acid and / or a soluble salt of chloroiridic acid;

[0034] The organic solvent includes one or more of 1,2-propylene glycol, glycerol, benzyl alcohol, N,N-dimethylformamide and N,N-dimethylacetamide.

[0035] Optionally, the reaction conditions include: temperature of 140-180° C. and time of 3-8 h.

[0036] Optionally, the molar ratio of the TiO2-coated TiN, the surfactant and the iridium source calculated as chloroiridic acid is 1:(5-15):(0.2-0.4);

[0037] In the material obtained by the contact, the concentration of the iridium source calculated as iridium element is 0.001-0.01 mol / L.

[0038] A sixth aspect of the present disclosure provides an iridium-containing catalyst prepared by the method described in the fifth aspect of the present disclosure.

[0039] The seventh aspect of the present disclosure provides the use of the iridium-containing catalyst described in the first aspect or the sixth aspect of the present disclosure, or the TiO2-coated TiN described in the second aspect or the fourth aspect in a water electrolysis anode catalyst.

[0040] An eighth aspect of the present disclosure provides a proton exchange membrane water electrolysis device, comprising a proton exchange membrane, a cathode catalyst layer, an anode catalyst layer, a cathode diffusion layer and an anode diffusion layer, wherein the anode catalyst layer comprises the iridium-containing catalyst described in the first aspect or the sixth aspect.

[0041] A ninth aspect of the present disclosure provides a method for producing hydrogen by electrolyzing water, using the iridium-containing catalyst described in the first aspect or the sixth aspect, or using the proton exchange membrane water electrolysis device described in the eighth aspect.

[0042] Through the above technical scheme, the present invention uses TiO2-coated TiN as a carrier, which has a larger specific surface area and better electrical conductivity than pure TiO2 and pure TiN, which is beneficial to reducing the primary particle size of the active component, exposing more active sites, and thus improving the catalytic activity; compared with existing catalysts, the iridium-containing catalyst disclosed in the present invention has a lower overpotential, a higher mass specific activity, better cycle stability and a higher electrical conductivity, while having a lower iridium content.

[0043] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:

[0045] Figure 1 This is the XRD pattern of TiO2-coated TiN prepared in Example 1 of the present disclosure.

[0046] Figure 2 This is the XRD pattern of the commercial TiN support.

[0047] Figure 3TEM image of TiO2-coated TiN prepared in Example 2 of the present disclosure.

[0048] Figure 4 This is a comparison chart of the electrical conductivity of TiO2-coated TiN prepared in Example 3 of the present disclosure and commercial TiO2.

[0049] Figure 5 This is the OER performance diagram of the iridium-containing catalyst A3 prepared in Example 3 of the present disclosure. DETAILED DESCRIPTION

[0050] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.

[0051] In order to achieve the above-mentioned object, the present disclosure provides, in a first aspect, an iridium-containing catalyst, the iridium-containing catalyst comprising a carrier and an active component supported on the carrier;

[0052] The carrier includes TiN coated with TiO2, and the active component includes single substance Ir.

[0053] According to one embodiment of the present disclosure, the specific surface area of ​​the iridium-containing catalyst is 40-70 m 2 / g, preferably 50-60m 2 / g.

[0054] According to one embodiment of the present disclosure, the average particle size of the active component is 2-4 nm, preferably 2.1-3 nm.

[0055] According to one embodiment of the present disclosure, the conductivity of the iridium-containing catalyst is 0.005-0.03 S / mm.

[0056] According to one embodiment of the present disclosure, the content of the active component calculated as iridium element is 30-50% by weight, preferably 35-40% by weight, relative to the total weight of the iridium-containing catalyst. The iridium-containing catalyst of the present disclosure can reduce the usage of precious metal iridium while having a higher catalytic activity.

[0057] The second aspect of the present disclosure provides a carrier for anode catalyst for water electrolysis, wherein the carrier is TiN coated with TiO2, and the specific surface area of ​​the carrier is 100-150m 2 / g.

[0058] There is a strong interaction between the TiN and TiO2 in the TiO2-coated TiN disclosed in the present invention, and it has the advantages of excellent conductivity and large specific surface area. The catalyst prepared by loading elemental iridium thereon has the properties of resistance to high pressure, strong acid and high conductivity; TiO2 is an amorphous phase, and has a larger specific surface area and better conductivity than anatase TiO2, which is beneficial to further improve the catalytic activity of the prepared catalyst.

[0059] According to one embodiment of the present disclosure, the specific surface area of ​​the carrier is 120-140m 2 The TiO2-coated TiN with the above-mentioned specific surface area is beneficial to improving the dispersibility of the active component on its surface, and obtaining a catalyst loaded with a small-sized iridium active component, which can have high catalytic activity, cycle stability and conductivity when used in proton exchange membrane water electrolysis reaction.

[0060] According to one embodiment of the present disclosure, relative to the total weight of TiO2-coated TiN, the content of TiO2 is 40-60 wt%, and the content of TiN is 40-60 wt%; preferably, the content of TiO2 is 48-58 wt%, and the content of TiN is 42-52 wt%; the above content range is beneficial to simultaneously ensure a large surface area and conductivity of the carrier, and can further improve the catalytic activity of the prepared catalyst.

[0061] In the present disclosure, TiN has a face-centered cubic crystal type.

[0062] According to one embodiment of the present disclosure, the conductivity of the carrier is 1×10 -7 to 1.5×10 -6 S / mm.

[0063] According to one embodiment of the present disclosure, in the XRD spectrum of TiO2-coated TiN, there is no characteristic peak of TiO2, and the position of the characteristic peak of TiN is shifted to a high angle by 0.2-0.3 eV relative to the characteristic peak of pure TiN, and the lattice spacing corresponding to its (111) crystal plane is reduced to 0.243 nm, which is smaller than 0.245 nm of pure TiN, wherein "characteristic peak" refers to the diffraction peak, and "characteristic peak without TiO2" refers to the characteristic peak without crystalline TiO2; the above characterization data indicate that there is a strong synergistic effect between TiO2 and TiN.

[0064] In the present disclosure, in "TiO 2 coated TiN", TiO 2 may completely coat TiN or may be partially coated with TiN, preferably completely coated.

[0065] A third aspect of the present disclosure provides a method for preparing TiO2-coated TiN, the method comprising the following steps:

[0066] S1, mixing a complexing agent, a titanium source, TiN and water, adjusting the pH value of the mixture to 8-10 and performing a hydrolysis reaction to obtain a first material;

[0067] S2, heat treating the solid in the first material;

[0068] The complexing agent includes an organic polyacid.

[0069] The present invention adopts the method of adding a complexing agent to help adjust the hydrolysis rate of the titanium source and effectively reduce the excessive aggregation of the catalyst during the calcination process.

[0070] In the present disclosure, all washing methods are conventional in the art and can achieve the purpose of washing the solid and liquid cleanly, for example, ultrasonic washing.

[0071] In the present disclosure, all solid-liquid separation methods are conventional in the art and can achieve the purpose of solid-liquid separation. For example, rotary evaporation, centrifugal separation, etc. When the solid-liquid separation method is rotary evaporation, the temperature is 50-70°C; when the solid-liquid separation method is centrifugal separation, the speed of centrifugal separation is 9000-10000rpm, and the time is 5-20min.

[0072] According to one embodiment of the present disclosure, the complexing agent includes one or more organic polyacids having 2 to 10 carbon atoms, preferably one or more of ethylenediaminetetraacetic acid, oxalic acid, maleic acid and citric acid.

[0073] According to one embodiment of the present disclosure, the titanium source includes titanium salt and / or titanate, preferably one or more of titanium sulfate, ethyl titanate and tetrabutyl titanate.

[0074] According to one embodiment of the basic disclosure, the average particle size of TiN is 10-20 nm.

[0075] According to one embodiment of the present disclosure, in step S1, the conditions for the hydrolysis reaction include: time is 3-10 hours, temperature is 60-100°C; preferably, time is 4-6 hours, temperature is 80-90°C.

[0076] According to one embodiment of the present disclosure, in step S1, the mixing method can be, for example, heating and stirring, the time is 0.5-2h, preferably 1-1.5h; the temperature is 60-100°C, preferably 80-90°C; the above operation can promote the full mixing of the complexing agent and the titanium source, and further promote the formation of the complex.

[0077] According to one embodiment of the present disclosure, in step S1, the method for adjusting the pH value of the mixture may be, for example, adding one or more of sodium carbonate, sodium bicarbonate and sodium hydroxide to the raw material mixture, and the above substances may be added in the form of an aqueous solution.

[0078] In the present disclosure, pH values ​​are all values ​​measured at 25°C.

[0079] According to one embodiment of the present disclosure, in step S1, the molar ratio of the titanium source, TiN and the complexing agent in terms of titanium element is 1:(0.5-1.2):(0.5-2), preferably 1:(0.8-1.1):(1-1.5). The above ratio helps to adjust the hydrolysis rate of the titanium source and effectively reduce excessive aggregation of the catalyst during the calcination process.

[0080] According to one embodiment of the present disclosure, in step S1, in the mixture, the concentration of the titanium source calculated as titanium element is 0.1-1 mol / L, preferably 0.2-0.5 mol / L.

[0081] According to an embodiment of the present disclosure, step S2 further includes: performing solid-liquid separation on the first material; the solid-liquid separation method is preferably rotary evaporation.

[0082] According to one embodiment of the present disclosure, step S2 also includes: drying the solid material obtained by solid-liquid separation, and the drying method is conventional in the art, for example, an oven can be used for drying; the drying conditions include: temperature of 90-120°C, preferably 100-110°C; time of 6-20h, preferably 10-12h.

[0083] According to an embodiment of the present disclosure, step S2 further includes: grinding the solid after drying, and grinding can reduce the particle size of the precursor to make the calcination more complete.

[0084] According to one embodiment of the present disclosure, in step S2, the heat treatment method is roasting, and the roasting conditions include: time is 2-8h, preferably 2.5-6h, and further preferably 3-4h; temperature is 300-600°C, preferably 400-500°C; heating rate is 2-5°C / min, and the roasting atmosphere includes an air atmosphere with an oxygen content of 20-25% by volume.

[0085] According to one embodiment of the present disclosure, the method further comprises: washing the solid obtained by roasting for the first time, solid-liquid separation, washing for the second time, solid-liquid separation and drying. The washing method may be ultrasonic washing. The solvent used for the first washing is preferably water. The solvent used for the second washing is preferably a mixed solution of alcohol and water. The alcohol is preferably one or more of methanol, ethanol, n-propanol and isopropanol, more preferably ethanol. The volume ratio of ethanol to water is 1: (0.5-1.5), preferably 1: (0.6-1). When the pH value of the solvent after washing is detected to be neutral (25°C), the process is terminated. The drying method after solid-liquid separation is conventional in the art, such as drying overnight at 20-100°C in a vacuum drying oven.

[0086] A fourth aspect of the present disclosure provides TiO2-coated TiN prepared by the method described in the third aspect of the present disclosure.

[0087] The above-mentioned TiO2-coated TiN has the same characteristics as the TiO2-coated TiN described in the second aspect of the present disclosure, which will not be described in detail here.

[0088] A fifth aspect of the present disclosure provides a method for preparing an iridium-containing catalyst, the method comprising: contacting the TiO2-coated TiN, a surfactant, and an iridium source according to the second aspect or the fourth aspect of the present disclosure with an organic solvent to react;

[0089] The organic solvent includes one or more of saturated polyols, aromatic alcohols and amides.

[0090] According to one embodiment of the present disclosure, the surfactant includes an organic ammonium salt having 12-19 carbon atoms, preferably including one or more of cetyltrimethylammonium chloride, tetradecyltrimethylammonium bromide and cetyltrimethylammonium bromide.

[0091] According to one embodiment of the present disclosure, the iridium source includes chloroiridic acid and / or a soluble salt of chloroiridic acid; the iridium source can be added in the form of a compound or in the form of an aqueous solution.

[0092] According to one embodiment of the present disclosure, the organic solvent includes one or more of a saturated polyol having 2-5 carbon atoms, an aromatic alcohol having 6-10 carbon atoms, and an amide having 3-6 carbon atoms, and preferably includes one or more of 1,2-propylene glycol, glycerol, benzyl alcohol, N,N-dimethylformamide, and N,N-dimethylacetamide.

[0093] According to one embodiment of the present disclosure, contacting TiO2-coated TiN, a surfactant, an iridium source and an organic solvent comprises:

[0094] a. Mixing TiO2-coated TiN, a surfactant and an organic solvent;

[0095] b. Mixing the iridium source with the mixed material obtained in step a; wherein steps a and b are preferably carried out under stirring to ensure uniform mixing, and the stirring time is 1-2h.

[0096] According to one embodiment of the present disclosure, the reaction is preferably carried out by reflux, and the conditions include a temperature of 140-180°C and a time of 3-8h; preferably, a temperature of 150-170°C and a time of 4-6h; the above reflux can be carried out in an oil bath.

[0097] According to one embodiment of the present disclosure, the molar ratio of TiO2-coated TiN, surfactant and iridium source calculated as chloroiridic acid is 1:(5-15):(0.2-0.4); preferably 1:(6-10):(0.22-0.3); the above ratio helps to evenly disperse the active components on the carrier.

[0098] According to one embodiment of the present disclosure, in the material obtained by contact, the concentration of the iridium source calculated as iridium element is 0.001-0.01 mol / L, preferably 0.002-0.005 mol / L.

[0099] According to one embodiment of the present disclosure, the method further includes: subjecting the mixture obtained after the reaction to a first solid-liquid separation, washing, a second solid-liquid separation and drying. The washing method may be ultrasonic washing. The solvent used for washing is preferably a mixed solution of alcohol and water. The alcohol is preferably one or more of methanol, ethanol, n-propanol and isopropanol, more preferably ethanol. The volume ratio of ethanol to water is 1: (0.5-1.5), preferably 1: (0.6-1). The process is terminated when the pH value (25°C) of the solvent after washing is detected to be neutral. The drying method after solid-liquid separation is conventional in the art, such as drying overnight at 20-100°C in a vacuum drying oven. Using a mixed solution of water and alcohol as a detergent is beneficial for separating the catalyst from the aqueous phase.

[0100] A sixth aspect of the present disclosure provides an iridium-containing catalyst prepared by the method described in the fifth aspect of the present disclosure.

[0101] The above-mentioned iridium-containing catalyst has the same characteristics as the iridium-containing catalyst described in the first aspect of the present disclosure, which will not be described in detail here.

[0102] The seventh aspect of the present disclosure provides the use of the iridium-containing catalyst described in the first aspect or the sixth aspect of the present disclosure, or the TiO2-coated TiN described in the second aspect or the fourth aspect in a water electrolysis anode catalyst.

[0103] An eighth aspect of the present disclosure provides a proton exchange membrane water electrolysis device, comprising a proton exchange membrane, a cathode catalyst layer, an anode catalyst layer, a cathode diffusion layer and an anode diffusion layer, wherein the anode catalyst layer comprises the iridium-containing catalyst described in the first aspect or the sixth aspect.

[0104] A ninth aspect of the present disclosure provides a method for producing hydrogen by electrolyzing water, using the iridium-containing catalyst described in the first aspect or the sixth aspect, or using the proton exchange membrane water electrolysis device described in the eighth aspect.

[0105] The present invention will be described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form.

[0106] Unless otherwise specified, the raw materials used in the examples and comparative examples were obtained from commercial sources and were of analytical grade.

[0107] Instruments, methods and conditions for XRD analysis: X-ray diffraction analysis (XRD) was carried out on a Shimadzu X-ray diffractometer model XRD-6000. The test conditions included: tube voltage 40 kV, tube current 40 mA, Cu target Kα radiation, and 2θ scanning range 5° to 80°.

[0108] Instruments, methods and conditions for OER testing: The electrochemical workstation model is PARSTAT3000A-DX, and the rotating disk electrode model is 636A. A three-electrode system is used, with a saturated calomel electrode as the reference electrode, a platinum sheet as the counter electrode, and a glassy carbon electrode as the working electrode. The electrolyte used under acidic conditions is a 0.5M H2SO4 solution. The catalyst to be tested is ultrasonically uniformly dispersed in a mixed solution of isopropanol, water and Nafion, and then dripped onto the surface of the glassy carbon electrode. After natural drying, the working electrode is obtained, and the catalyst loading is 0.38 mg cm -2 The test temperature was 25°C. Before the test, oxygen was passed through for 30 minutes to saturate the solution with oxygen. The rotation speed was 2500 rpm. The scanning range of the linear polarization curve was 1.2V-1.5V (vs RHE) and the scanning rate was 5mV / s. The stability test scanning range was 1.26V-1.56V (vs RHE), the scanning rate was 50mV / s, and the number of cycles was 10,000.

[0109] Instruments, methods and conditions for specific surface area test: BET specific surface area was measured on the ASAP2420 physical adsorption instrument of Mack Instruments, USA. The test conditions include: firstly, sample pretreatment was performed, a certain amount of sample was weighed and loaded into a sample tube that had been tested with a blank, and then placed in a degassing treatment unit, vacuumed, and degassed for 6 hours at a furnace temperature of 300°C and a vacuum degree of less than 1.33 Pa. Then, the sample was measured, the treated sample tube was loaded into the measurement unit, the Dewar flask was filled with liquid nitrogen, and the measurement and calculation were performed. The adsorption isotherm was measured by the static volumetric method, the pore size distribution was calculated by the BJH method, and the specific surface area was calculated by the BET formula.

[0110] The average particle size test method and conditions are as follows: The average particle size is calculated based on the measured XRD pattern according to the Scherrer formula.

[0111] Instrument, method and conditions for TEM analysis: The transmission electron microscope (TEM) used in the present invention is a JEM-2100 (TEM) (Japan Electron Co., Ltd.), and the transmission electron microscope test conditions are: the acceleration voltage is 200 kV.

[0112] Instruments, methods and conditions for conductivity analysis: The conductivity was measured on the FT-301B-200KG automatic powder resistivity tester of ROOKO Ruikewei Company, with the automatic pressure set to 200kg, the constant pressure time to 10s, and the cross-sectional area of ​​the cylinder to 78.5mm 2 , with a diameter of 10 mm, and weigh about 0.2 g of sample for testing.

[0113] Testing method for TiO2 content in carrier: The TiO2 content in carrier is calculated by the dosage of titanium source.

[0114] Test method for TiN content in carrier: The TiN content in the carrier is calculated by the TiN content added during preparation.

[0115] Testing method for the content of active components in the catalyst: The present invention uses inductively coupled plasma mass spectrometry (ICP-MS) to test the Ir ion content in the reaction solution after TiO2-coated TiN loaded with iridium, and obtains the iridium content in the catalyst through conversion. The model of ICP-MS is VISTA-710ES (Varian, USA).

[0116] Source of commercial TiN: Aladdin Reagent (Shanghai) Co., Ltd., particle size is 10-20 nm.

[0117] Source of commercial TiO2: Shanghai McLean Biochemical Technology Co., Ltd., the crystal form is anatase.

[0118] Example 1

[0119] The iridium-containing catalyst A1 was prepared by the following steps:

[0120] (1) Mix 3.6 g (15 mmol) of titanium sulfate, 0.93 g (15 mmol) of TiN, and 4.3 g (22.5 mmol) of citric acid with 50 mL of water and stir at 90 °C for 1 h;

[0121] (2) adding Na2CO3 solution (concentration of 2 mol / L) dropwise to the raw material mixture obtained in step (1) to adjust the pH value of the solution to 8-9, and performing a hydrolysis reaction at 90°C for 4 hours to obtain a first material;

[0122] The molar ratio of the titanium source, TiN and the complexing agent calculated as titanium element is 1:1:1.5, and the concentration of the titanium source calculated as titanium element in the mixture is 0.3 mol / L;

[0123] (3) cooling the first material, rotary evaporating it at 70° C., and drying it in an oven at 100° C. overnight;

[0124] (4) The dried solid was cooled and ground, and then laid flat on a porcelain boat. The solid was heated to 500° C. at a heating rate of 2° C. / min in an air atmosphere (oxygen volume fraction of 21%) for 3 h.

[0125] (5) The calcined solid was cooled to room temperature, first ultrasonically washed with deionized water and then centrifuged (10000 rpm, 10 min), then washed with a mixed solution of ethanol and water in a volume ratio of 1:1, centrifuged (10000 rpm, 10 min), and the supernatant was discarded, and the above steps were repeated until the pH at 25°C was neutral; dried in a vacuum drying oven at 100°C overnight, and ground to obtain TiO2-coated TiN, the parameters of which are listed in Table 1;

[0126] (6) 80 mg (1.12 mmol) of the TiO2-coated TiN prepared above, 2.24 g (7 mmol) of hexadecyltrimethylammonium chloride (CTAC) and 80 mL of 1,2-propylene glycol solvent were mixed and stirred for 1 h;

[0127] (7) adding 1.43 mL of aqueous chloroiridic acid solution (containing 0.26 mmol of chloroiridic acid) to the mixture obtained in step (6), stirring for 2 h, and then refluxing in an oil bath at 160° C. for 4 h;

[0128] The molar ratio of TiO2-coated TiN, CTAC and the iridium source calculated as chloroiridic acid is 1:6.25:0.23, and the concentration of the iridium source calculated as iridium element in the material of step (7) is 0.003 mol / L;

[0129] (8) cooling to room temperature, centrifuging to obtain a solid product, adding a mixed solution of water and ethanol, wherein the volume ratio of water to ethanol is 1:1, ultrasonic washing, and then centrifuging at a centrifugal speed of 10000 rpm for 5 min. After centrifugation, the supernatant is discarded, and the above steps are repeated until the pH at 20° C. is neutral, and the washing process is completed;

[0130] (9) The washed solid was placed in a vacuum drying oven and dried at 30° C. overnight. The iridium-containing catalyst A1 was obtained by grinding. The parameters of the catalyst A1 are listed in Table 1.

[0131] XRD test was performed on the TiO2-coated TiN prepared in Example 1. The results are as follows: Figure 1 .

[0132] XRD test results of commercial TiN carrier are as follows: Figure 2 .

[0133] Example 2

[0134] The iridium-containing catalyst A2 was prepared by the method of Example 1, except that in step (2), the pH was adjusted to 9-10. The parameters of the TiO2-coated TiN and the iridium-containing catalyst A2 are listed in Table 1.

[0135] The TiO2-coated TiN prepared in Example 2 was subjected to TEM test, and the results are as follows: Figure 3 .

[0136] Example 3

[0137] The iridium-containing catalyst A3 was prepared by the method of Example 1, except that the amount of citric acid used was 2.8 g (15 mmol), the molar ratio of the titanium source, titanium nitride and the complexing agent was 1:1:1, and the parameters of the TiO2-coated TiN and the iridium-containing catalyst A3 are listed in Table 1.

[0138] The conductivity of TiO2-coated TiN prepared in Example 3 was compared with that of commercial TiO2. The results are as follows: Figure 4 .

[0139] The OER performance of catalyst A3 prepared in Example 3 was tested. The results are as follows: Figure 5 .

[0140] Example 4

[0141] Catalyst A4 was prepared by the method of Example 1, except that the calcination temperature was 400° C. and the calcination time was 4 h. The parameters of the TiO2-coated TiN and iridium-containing catalyst A4 are listed in Table 1.

[0142] Example 5

[0143] Catalyst A5 was prepared by the method of Example 1, except that the molar ratio of the titanium source, TiN and the complexing agent calculated on the basis of titanium element was 1:3:1.5. The parameters of the TiO2-coated TiN and the iridium-containing catalyst A5 are listed in Table 1.

[0144] Example 6

[0145] The iridium-containing catalyst A6 was prepared by the following steps:

[0146] (1) Ethyl titanate (10 mmol), TiN (10 mmol) and citric acid (10 mmol) were mixed with 50 mL of water and stirred at 80 °C for 1 h;

[0147] (2) adding Na2CO3 solution (concentration of 2 mol / L) dropwise to the raw material mixture obtained in step (1) to adjust the pH value of the solution to 8-9, and performing a hydrolysis reaction at 80°C for 5 hours to obtain a first material;

[0148] The molar ratio of the titanium source, TiN and the complexing agent calculated as titanium element is 1:1:1, and the concentration of the titanium source calculated as titanium element in the mixture is 0.2 mol / L;

[0149] (3) cooling the first material, rotary evaporating it at 70° C., and drying it in an oven at 100° C. overnight;

[0150] (4) The dried solid was cooled and ground, and then laid flat on a porcelain boat. The solid was heated to 450° C. at a heating rate of 3° C. / min in an air atmosphere (oxygen volume fraction 21%) for 4 h.

[0151] (5) The calcined solid was cooled to room temperature, first ultrasonically washed with deionized water and then centrifuged (10000 rpm, 10 min), then washed with a mixed solution of ethanol and water in a volume ratio of 1:1, centrifuged (10000 rpm, 10 min), and the supernatant was discarded, and the above steps were repeated until the pH at 25°C was neutral; dried in a vacuum drying oven at 100°C overnight, and ground to obtain TiO2-coated TiN, the parameters of which are listed in Table 1;

[0152] (6) 50 mg (0.7 mmol) of the TiO2-coated TiN prepared above, 2.24 g (7 mmol) of hexadecyltrimethylammonium chloride (CTAC) and 80 mL of N,N-dimethylformamide solvent were mixed and stirred for 2 h;

[0153] (7) adding 1.43 mL of aqueous chloroiridic acid solution (containing 0.26 mmol of chloroiridic acid) to the mixture obtained in step (6), stirring for 2 h, and then refluxing in an oil bath at 165 ° C for 5 h;

[0154] The molar ratio of TiO2-coated TiN, CTAC and the iridium source calculated as chloroiridic acid is 1:10:0.37, and the concentration of the iridium source calculated as iridium element in the material of step (7) is 0.003 mol / L;

[0155] (8) cooling to room temperature, centrifuging to obtain a solid product, adding a mixed solution of water and ethanol, wherein the volume ratio of water to ethanol is 1:1, ultrasonic washing, and then centrifuging at a centrifugal speed of 10000 rpm for 5 min. After centrifugation, the supernatant is discarded, and the above steps are repeated until the pH at 25° C. is neutral, and the washing process is completed;

[0156] (9) The washed solid was placed in a vacuum drying oven and dried at 30° C. overnight. The iridium-containing catalyst A6 was obtained by grinding. The parameters of the catalyst A6 are listed in Table 1.

[0157] The catalysts prepared in Examples 1-6 were subjected to XRD testing. In the spectra, there was no characteristic peak of TiO2, and the position of the characteristic peak of TiN was shifted toward a higher angle by 0.2-0.3 eV relative to the characteristic peak of pure TiN.

[0158] Comparative Example 1

[0159] The iridium-containing catalyst D1 was prepared by the method of Example 1, except that commercial titanium dioxide was used as a carrier, and the molar ratio of the titanium dioxide carrier, CTAC and the iridium source calculated as chloroiridic acid was 1:6.3:0.42. The parameters are listed in Table 1.

[0160] Comparative Example 2

[0161] (1) Weigh 1.2 g (15 mmol) of TiO2 and 0.93 g (15 mmol) of TiN and mix with 50 mL of ethanol, and stir at room temperature (25°C) overnight;

[0162] (2) centrifuging the mixed solution (10000 rpm, 10 min), drying the obtained solid in a vacuum drying oven overnight, and grinding to obtain a carrier TiO2-TiN;

[0163] (3) 80 mg (1 mmol) of the TiO2-TiN carrier prepared above, 2.24 g (7 mmol) of CTAC and 80 mL of 1,2-propylene glycol solvent were mixed and stirred for 1 h;

[0164] (4) adding 1.43 mL of aqueous chloroiridic acid solution (containing 0.26 mmol of chloroiridic acid) to the mixture obtained in step (3), stirring for 2 h, and then refluxing in an oil bath at 160° C. for 4 h;

[0165] The molar ratio of the TiO2-TiN carrier, CTAC and chloroiridic acid is 1:6.25:0.23, and the concentration of iridium in the material of step (4) is 0.003 mol / L;

[0166] (5) cooling to room temperature, centrifuging to obtain a solid product, adding a mixed solution of water and ethanol, wherein the volume ratio of water to ethanol is 1:1, ultrasonic washing, and then centrifuging at a centrifugal speed of 10000 rpm for 5 min. After centrifugation, the supernatant is discarded, and the above steps are repeated until the pH at 25° C. is neutral, and the washing process is completed;

[0167] (6) The washed solid was placed in a vacuum drying oven, dried overnight, and ground to obtain the iridium-containing catalyst D2.

[0168] Comparative Example 3

[0169] Commercial iridium black catalyst was used, and the manufacturer was Alfa Company of the United Kingdom.

[0170] Comparative Example 4

[0171] Commercial iridium dioxide catalyst is used, and the manufacturer is Chunhua Hydrogen Energy Technology Co., Ltd.

[0172] Comparative Example 5

[0173] The iridium-containing catalyst D5 was prepared by the method of Example 1, except that commercial TiN was used as a carrier, and the molar ratio of TiN, CTAC and chloroiridic acid was 1:6.3:0.32. The parameters are listed in Table 1.

[0174] Test Example 1-11

[0175] A three-electrode system is used, the reference electrode is a saturated calomel electrode, the counter electrode is a platinum sheet, and the working electrode is a glassy carbon electrode. The electrolyte used under acidic conditions is a 0.5M H2SO4 solution. The catalysts A1-A6 prepared in the examples, the catalysts D1-D2 and D5 prepared in the comparative examples, the commercial iridium black catalyst D3, and the commercial iridium dioxide catalyst D4 are uniformly dispersed in a mixed solution of 0.7mL isopropanol, 0.3mL water, and 10μL 5wt% Nafion solution (perfluorosulfonic acid polymer solution) by ultrasonic means (the mass ratio of the catalyst to Nafion is 10:1), coated on the surface of the glassy carbon electrode, and the working electrode is obtained after natural drying. Before the test, oxygen is passed through for 30min to saturate the solution with oxygen. The scanning interval of the linear polarization curve is 1.2-1.5V (vsRHE) and the scanning rate is 5mV / s. The stability test scanning interval is 1.26-1.56V (vs RHE) and the scanning rate is 50mV / s. The test results are listed in Table 1.

[0176] Table 1

[0177]

[0178]

[0179] from Figure 1 It can be seen that the TiO2-coated TiN prepared in the present invention has inconspicuous broad peaks at 2θ=25.3° and 48.0°, indicating that the TiO2 in the carrier is an amorphous phase; diffraction peaks appear at 2θ=36.9°, 42.9° and 62.2°, corresponding to the face-centered cubic crystal form of TiN, and the lattice spacing corresponding to the (111) plane is 0.243nm.

[0180] from Figure 2 It can be seen that the commercial TiN carrier has sharp diffraction peaks at 2θ=36.6°, 42.9° and 62.2°, and the lattice spacing corresponding to the (111) plane is 0.245 nm.

[0181] Further, through Figure 1 and Figure 2 It can be seen from the comparison that in the XRD pattern of TiO2-coated TiN prepared in the present invention, the position of the TiN characteristic peak is shifted to a high angle by 0.2-0.3 eV relative to the characteristic peak of pure TiN, and the lattice spacing corresponding to its (111) crystal plane is reduced to 0.243 nm, which is smaller than 0.245 nm of pure TiN. There is a strong synergistic effect between TiO2 and TiN.

[0182] from Figure 3 It can be seen that the TiO2-coated TiN prepared in the present disclosure is a composite structure of amorphous TiO2 nanosheets coating TiN particles.

[0183] from Figure 4 It can be seen that the TiO2-coated TiN prepared in the present disclosure has a higher conductivity than commercial TiO2.

[0184] from Figure 5 It can be seen that the iridium-containing catalyst prepared in the present disclosure still has a low acidic OER overpotential of only 220 mV@10 mA / cm when the Ir content is reduced to 38%. 2 .

[0185] According to the data in Table 1, the TiO2-coated TiN prepared by the method disclosed in the present invention has the advantages of excellent electrical conductivity and large specific surface area, which is conducive to the preparation of catalysts with smaller active components. The conductivity of the composite carrier is much higher than that of commercial titanium oxide, which is conducive to reducing the content of precious metals in the membrane electrode. While reducing the amount of precious metal iridium, it has the advantages of lower overpotential than pure iridium dioxide (D4), significantly higher mass specific activity than pure iridium dioxide (D4) and iridium black (D3), and significantly better cycle stability than iridium black (D3). When it is used as an anode catalyst for proton exchange membrane water electrolysis to produce hydrogen, it has the characteristics of low overpotential, high activity, good cycle stability and high conductivity.

[0186] Further, according to the comparison between Examples 1-4 and Examples 5-6, it can be seen that the catalyst activity can be further optimized by adjusting the ratio of TiO2 and TiN in the carrier, the loading of the iridium active component, etc. According to the comparison between Examples 1-4 and Comparative Example 1, when a single commercial titanium dioxide granular carrier is used, when the iridium content is high, the overpotential, mass specific activity and stability of the prepared catalyst are worse than those of the catalyst of the present application; according to the comparison between Examples 1-4 and Comparative Example 2, when TiN-TiO2 prepared by mechanical mixing is used as a carrier, due to the weak interaction between TiO2 and TiN, the overpotential, mass specific activity and stability of the prepared catalyst are worse than those of the iridium-containing catalyst prepared in the present disclosure; according to the comparison between Examples 1-4 and Comparative Example 5, it can be seen that when a single commercial titanium nitride granular carrier is used, when the iridium content is high, the overpotential and mass specific activity of the prepared catalyst are worse than those of the catalyst of the present application.

[0187] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.

[0188] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

[0189] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.

Claims

1. An iridium-containing catalyst, It is characterized in that The iridium-containing catalyst comprises a carrier and an active component supported on the carrier; The support includes TiO 2 The coated TiN, the active component includes single substance Ir.

2. The iridium-containing catalyst according to claim 1, in, The specific surface area of ​​the iridium-containing catalyst is 40-70 m 2 / g; The average particle size of the active component is 2-4 nm; Optionally, the conductivity of the iridium-containing catalyst is 0.005-0.03 S / mm.

3. The iridium-containing catalyst according to claim 1, in, The content of the active component calculated as iridium element is 30-50 weight % relative to the total weight of the iridium-containing catalyst.

4. A carrier for anode catalyst for water electrolysis, It is characterized in that The carrier is TiO 2 The coated TiN, the specific surface area of ​​the carrier is 100-150m 2 / g.

5. The vector according to claim 4, in, Compared with the TiO 2 The total weight of the coated TiN, the TiO 2 The content of is 40-60 wt %, and the content of TiN is 40-60 wt %; The TiN is a face-centered cubic crystal; The conductivity of the carrier is 1×10 -7 to 1.5×10 -6 S / mm.

6. The vector according to claim 4, in, In the TiO 2 In the XRD spectrum of coated TiN, there is no TiO 2 The characteristic peak of TiN is shifted toward a high angle by 0.2-0.3 eV relative to the characteristic peak of pure TiN.

7. Preparation of TiO 2 TiN coating method, It is characterized in that The method comprises the following steps: S1, mixing a complexing agent, a titanium source, TiN and water, adjusting the pH value of the mixture to 8-10 and performing a hydrolysis reaction to obtain a first material; S2, heat treating the solid in the first material; The complexing agent includes an organic polyacid.

8. The method according to claim 7, in, The complexing agent includes one or more organic polyacids having 2 to 10 carbon atoms, preferably one or more of ethylenediaminetetraacetic acid, oxalic acid, maleic acid and citric acid; The titanium source includes one or more of titanium sulfate, ethyl titanate and tetrabutyl titanate; Optionally, the particle size of the TiN is 10-20 nm.

9. The method according to claim 7, in, In step S1, the conditions of the hydrolysis reaction include: time of 3-10h, temperature of 60-100°C; The mixing conditions include: time of 0.5-2h, temperature of 60-100°C; The molar ratio of the titanium source, the TiN and the complexing agent calculated on the basis of titanium element is 1:(0.5-1.2):(0.5-2); In the mixture, the concentration of the titanium source calculated as titanium element is 0.1-1 mol / L.

10. The method according to claim 7, in, In step S2, the heat treatment method is roasting, and the roasting conditions include: time of 2-8h, temperature of 300-600°C, heating rate of 2-5°C / min, and roasting atmosphere including air atmosphere with oxygen content of 20-25% by volume.

11. TiO prepared by the method according to any one of claims 7 to 10 2 Coated TiN.

12. A method for preparing an iridium-containing catalyst, It is characterized in that The method comprises: treating the TiO 2 The coated TiN, the surfactant, the iridium source and the organic solvent are contacted to react; The organic solvent includes one or more of saturated polyols, aromatic alcohols and amides.

13. The method according to claim 12, in, The surfactant comprises an organic ammonium salt having 12 to 19 carbon atoms, preferably comprising one or more of cetyltrimethylammonium chloride, tetradecyltrimethylammonium bromide and cetyltrimethylammonium bromide; The iridium source includes chloroiridic acid and / or a soluble salt of chloroiridic acid; The organic solvent includes one or more of 1,2-propylene glycol, glycerol, benzyl alcohol, N,N-dimethylformamide and N,N-dimethylacetamide.

14. The method according to claim 12, in, The reaction conditions include: temperature of 140-180° C. and time of 3-8 h.

15. The method according to claim 12, in, The TiO 2 The molar ratio of the coated TiN, the surfactant and the iridium source calculated as chloroiridic acid is 1:(5-15):(0.2-0.4); In the material obtained by the contact, the concentration of the iridium source calculated as iridium element is 0.001-0.01 mol / L.

16. An iridium-containing catalyst prepared by the method described in any one of claims 12 to 15.

17. The iridium-containing catalyst according to any one of claims 1 to 3 and 16, or the TiO2 according to any one of claims 4 to 6 and 11 2 Application of coated TiN in anode catalysts for water electrolysis.

18. A proton exchange membrane water electrolysis device, comprising a proton exchange membrane, a cathode catalyst layer, an anode catalyst layer, a cathode diffusion layer and an anode diffusion layer, It is characterized in that The anode catalyst layer comprises the iridium-containing catalyst according to any one of claims 1-3 and 16.

19. A method for producing hydrogen by electrolyzing water, It is characterized in that Use the iridium-containing catalyst described in any one of claims 1-3 and 16, or use the proton exchange membrane water electrolysis device described in claim 18.

Citation Information

Patent Citations

  • Sea urchin-like rutile titanium dioxide supported ruthenium oxide oxygen evolution catalyst, preparation method and application thereof

    CN109289843A

Cited By

  • Ir-doped WO3 (at) TiN as well as preparation method and application thereof

    CN120205198A

  • Ir-doped WO3@TiN, and a preparation method and application thereof

    CN120205198B