Carbon fiber high-temperature-resistant sizing agent for PPS thermoplastic composite material matrix and preparation method

Through the preparation method of water-based polyurethane high-temperature resistant sizing agent, the problem of low interlayer shear strength of CF/PPS thermoplastic composite materials is solved, the interface bonding strength and mechanical properties are improved, and it is suitable for high-temperature application fields such as aerospace and aerospace.

CN118814482APending Publication Date: 2024-10-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310425405.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The interlaminar shear strength of CF/PPS thermoplastic composites is low, resulting in weak interface interaction, poor wettability, and easy delamination failure, which affects the mechanical properties of the material.

Method used

A method for preparing a water-based polyurethane high-temperature resistant sizing agent is used to generate a polyurethane dispersion containing a hydrophilic structure through pre-polymerization, water dispersion, chain extension and cross-linking reaction steps, and an emulsion layer is formed on the surface of the carbon fiber to improve fiber and PPS The interfacial bonding strength of the matrix.

Benefits of technology

It significantly improves the interface shear strength of carbon fiber and PPS, increases the interlaminar shear strength of composite materials, improves the interface bonding between fiber and matrix, enhances the overall mechanical properties of the material, and is suitable for high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004187957420000031
    Figure BDA0004187957420000031
  • Figure BDA0004187957420000032
    Figure BDA0004187957420000032
Patent Text Reader

Abstract

The invention provides a carbon fiber high-temperature-resistant sizing agent for a PPS thermoplastic composite material matrix and a preparation method of the carbon fiber high-temperature-resistant sizing agent. The preparation method comprises four stages of prepolymerization, formation of an aqueous dispersion, a chain extension reaction and a cross-linking reaction, and the prepared sizing agent enables the interfacial shear strength (IFSS) of carbon fibers and PPS to reach 40-50 MPa, which is improved by 25-56% compared with the IFSS of non-sized carbon fibers. The method disclosed by the invention has the characteristics of high efficiency, environmental friendliness and capability of realizing large-scale production, and the prepared sizing agent can improve the interface strength during combination of inorganic materials and can be applied to the fields of aerospace, medical treatment, machinery, automobiles, rail transit, petroleum transportation and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon fiber reinforced polyphenylene sulfide (CF / PPS) composite materials, and specifically relates to a carbon fiber high temperature resistant sizing agent for a PPS thermoplastic composite matrix and a preparation method thereof. Background Art

[0002] Polyurethane (PU) is a heterochain polymer with characteristic functional groups of carbamate (-NHCOO-), usually polymerized from oligomer polyols, polyisocyanates and chain extenders. The main chain of the polyurethane molecule is composed of flexible long-chain polyols and rigid isocyanate blocks, and has the characteristics of microphase separation, which can effectively disperse stress. The coexistence of polar and non-polar segments in the molecular chain also improves the chemical stability of polyurethane. At the same time, the widespread hydrogen bonding in the polymer further improves the mechanical properties of the material. Therefore, polyurethane is a multifunctional and multi-purpose polymer material with excellent properties such as friction resistance, low temperature resistance, biocompatibility, toughness, and easy processing. It is widely used in many fields such as elastomers, plastics, coatings, and foams.

[0003] The isocyanate (-NCO) group of polyurethane is very active and can react with functional groups such as -OH and -COOH. It can be used as a surface treatment agent to treat the surface of inorganic materials to enhance the interfacial interaction between inorganic materials and polymer materials (such as polyurethane, polyphenylene sulfide, etc.) and improve interfacial bonding. For polyurethane materials, surface treatment agents are a very important type of additives. For special synthetic rubbers such as polyurethane elastomers, there is a great demand for high value-added additives. Based on the huge market for polyurethane, the prospects for the additive market are bright. In conjunction with the research and development and application of polyurethane materials, the industry needs to further carry out application research and promotion of polyurethane additives, and develop better and more varieties while focusing on energy conservation, environmental protection and application performance.

[0004] In recent years, thermoplastic composites have attracted wide attention due to their advantages of good recyclability, secondary processability, high impact toughness, high specific strength and high specific modulus. Among various thermoplastic composites, carbon fiber reinforced polyphenylene sulfide (CF / PPS) has excellent properties such as high stiffness, high thermal stability, chemical corrosion resistance, wear resistance, and biocompatibility. It is expected to be used as a structural material to replace metal or thermosetting composites with mature processes. It is widely used in aerospace, medical, machinery, automobile and rail transportation, oil transportation and other fields.

[0005] However, the actual application of CF / PPS thermoplastic composites is not optimistic. The main problem is that its interlaminar shear strength (ILSS) is low (the ILSS of thermosetting composites is usually more than 80MPa, while the ILSS of most CF / PPS thermoplastic composites is only 40-70MPa), and it is easy to delaminate and fail during use. The main reason for this performance defect is that the interface interaction between carbon fiber and PPS matrix is ​​weak and the wettability is very poor, which easily produces pores during the composite molding process. The fundamental reason is that CF has a relatively stable six-membered ring structure, and the surface is composed of non-polar and highly ordered graphite basal planes, so that the fiber surface contains fewer active functional groups, and the PPS melt viscosity is high, so the wettability between carbon fiber and PPS resin is poor, and the interface bonding strength is weak. As the link for load transfer between fiber and resin matrix, the bonding strength of the interface layer greatly affects the mechanical properties of the overall composite material. When a composite material with low interface strength is damaged, cracks extend along the interface, and the reinforcing effect of the fiber cannot be well exerted, so that the strength of the composite material is far lower than the theoretical value.

[0006] Surface modification of CF can solve the above problems and improve the interlaminar shear strength and other properties of composite materials. There are two types of known technologies, one is "activation" (sometimes also called oxidation), and the other is "sizing". It can be used alone or in combination. The principle of activation modification is to introduce active functional groups on the fiber surface, increase the number of chemical bonds or hydrogen bonds between the fiber and the polymer matrix, and improve the interfacial bonding strength of the composite material through powerful chemical action. The principle of sizing modification is to make a thin layer of polymer (which may be different from the matrix) adhere to the fiber surface through a solution or emulsion coating, and use its ability to simultaneously produce strong interactions with the fiber and the matrix to build a bridge between the fiber and the matrix that originally interacted weakly, thereby enhancing the correlation between the two.

[0007] Existing sizing technologies include reactive sizing agents and coating sizing agents. Reactive sizing agents (surface grafting, coupling agents, etc.) have a low reaction rate and need to be used in conjunction with the previous activation technologies. Coating sizing agents (relying on van der Waals forces) are easy to operate and can also improve the wettability of the matrix to the fiber, which is conducive to large-scale production. Summary of the invention

[0008] The present invention aims to provide a carbon fiber high temperature resistant sizing agent for a PPS thermoplastic composite material matrix and a preparation method thereof, wherein the prepared composite material has the advantages of high interlaminar shear strength. The preparation method of the present invention comprises the following steps:

[0009] (1) Prepolymerization stage: a slightly excessive amount of diisocyanate reacts with polyether diol or polyester diol to form a prepolymer terminated by an isocyanate (-NCO) group; a hydrophilic group is introduced into a compound with a hydrophilic group into a polyurethane (PU) prepolymer terminated by an isocyanate, and a catalyst is added to react to form a polyurethane prepolymer containing a hydrophilic structure;

[0010] (2) Water dispersion formation stage: adding a neutralizing agent and water to disperse the polyurethane prepolymer containing a hydrophilic structure in water to form an aqueous polyurethane dispersion;

[0011] (3) Chain extension reaction stage: adding highly active polyamine chain extenders to further extend the chains of the aqueous polyurethane dispersion in a dispersed state to obtain a polyurethane dispersion with a high relative molecular mass;

[0012] (4) Cross-linking reaction stage: Add some additives, such as cross-linking agents, wetting agents, etc., to start the cross-linking reaction and improve the temperature resistance and wettability of polyurethane.

[0013] Preferably, in the prepolymerization stage, under a nitrogen atmosphere, the reaction temperature is 70-75°C, and at the beginning of the reaction, an equivalent amount of diisocyanate is first added to react with the polyether diol or polyester diol, and the hydrogen of the alcohol hydroxyl group is added to the nitrogen atom of the isocyanate group, and the reaction has no by-products. During the reaction, a small amount of diisocyanate is gradually added, and the amount added is 1% to 10% of the amount of diisocyanate added at the beginning of the reaction, thereby forming a PU prepolymer terminated by an isocyanate (-NCO) group, and the reaction time is 2 to 3 hours. The general reaction formula is as follows:

[0014]

[0015] Formula 1: Reaction formula of isocyanate (-NCO) addition reaction

[0016] Introduce hydrophilic groups, add active hydrogen group compounds to react with the terminal -NCO to extend the chain, add catalysts (such as organic tin, organic bismuth, dibutyl dilauric acid, etc.) to catalyze the reaction, and react for about 3 to 4 hours to generate PU prepolymers containing hydrophilic structures. When the reaction time is too long, the molecular weight of the prepolymer is too large and the degree of polymerization is too high; when the reaction time is too short, the monomers have not yet been fully polymerized into prepolymers. The general reaction formula is as follows:

[0017]

[0018] Formula 2: Common compounds with active hydrogen groups react with isocyanate (-CNO)

[0019] In the preparation method as described above, at the stage of forming an aqueous dispersion, the content of the end group (-NCO) of the polyurethane prepolymer is measured. When it no longer changes, it means that the reaction is completed. The PU prepolymer molecular chain contains a hydrophilic group, which can be used as an internal emulsifier. A neutralizer and water are added to form an aqueous polyurethane dispersion dispersed in water. During the dispersion process, the viscosity of the system increases, and 10-15wt% of an organic solvent (including but not limited to acetone, dimethylformamide (DMF), N-methylpyrrolidone (NMP), etc.) can be added to reduce the viscosity of the polymer, and an external shear force is applied to facilitate uniform dispersion. When the PU molecular chain is emulsified and dispersed in water, since the -NCO group will react with water, the self-emulsification step time should not be too long, and the emulsification temperature should not be higher than the critical point temperature of the reaction between water and the -NCO group to reduce the occurrence of side reactions. Since emulsification itself is an exothermic reaction, if the emulsification temperature is too high or the time is too long, the -NCO in the system will react with water to generate substituted urea and gel. Therefore, preferably, the self-emulsification step time should be ≤30 minutes and the emulsification temperature should be ≤30°C to make the system smooth and reduce side reactions.

[0020] In the preparation method as described above, during the chain extension reaction stage, a highly active polyamine chain extender can be added to the polyurethane aqueous dispersion to adjust the ratio of soft and hard segments and the molecular weight in the polyurethane molecule, so that it can be further chain extended in a dispersed state to obtain a polyurethane dispersion with a high relative molecular mass. The addition amount is 2-6% of the mass of the polyurethane aqueous dispersion. However, the content of the chain extender is not necessarily the higher the better. As the content of the chain extender increases, the content of carboxyl groups in the aqueous polyurethane system increases, and the carboxyl groups easily react with H to produce hydrogen bonds, that is, the hydrogen bonding effect in the main chain is enhanced, and the cohesion is also improved, which ultimately leads to enhanced bonding strength. In the aqueous polyurethane emulsion, if the content of the chain extender is too high, the hard segment content of the polymer is too high, which easily leads to difficulty in the movement of the molecular chain and has an adverse effect on increasing the bonding strength.

[0021] In the preparation method described above, during the crosslinking reaction stage, the temperature resistance, water resistance and solvent resistance of the water-soluble polyurethane are relatively low, and the addition of some additives (such as crosslinking agents, wetting agents, etc.) is beneficial to improve these properties. Commonly used crosslinking agents are any one of organic peroxides, silanes, acrylic acid, acrylamide, hydroxyethyl acrylate, divinylbenzene, diisocyanate, N,N-methylenebisacrylamide (MBA), etc., or any combination thereof, and the addition amount is 1-4% of the mass of the polyurethane aqueous dispersion, and more preferably CA-01, CA-02, The wetting agent is any one of alkyl sulfates, sulfonates, fatty acids, carboxylic acid soaps, phosphates, polyoxyethylene alkylphenol ethers, polyoxyethylene fatty alcohol ethers, polyoxyethylene polyoxypropylene block copolymers, etc., or any combination thereof, and the addition amount is 0.5-2% of the mass of the polyurethane aqueous dispersion, and more preferably FS-640, PSA-96, Twin245, TEGO Dispers 688 or any combination thereof, the addition amount is 0.8-1.5% of the mass of the polyurethane aqueous dispersion.

[0022] The sizing agent is prepared by the preparation method of the carbon fiber high temperature resistant sizing agent for the PPS thermoplastic composite matrix. The static contact angle between the sizing agent and the carbon fiber is 15-21°, and the mass loss at 330°C is 8-29%. The interfacial shear strength (IFSS) between the sizing carbon fiber and PPS reaches 40-50MPa, which is 25-56% higher than the IFSS of the unsized carbon fiber (32MPa).

[0023] Due to the adoption of the above technical solution, the present invention has the following beneficial effects:

[0024] The waterborne polyurethane prepared by the present invention generally does not use organic solvents or a small amount of solvents, has little impact on human health and less harm to the environment. Compared with the external emulsification method, the internal emulsification method only requires a very small shear force and does not require an emulsifier. The polyurethane prepolymer with a hydrophilic group can self-emulsify, so that the polyurethane is evenly dispersed in water, and the product stability is better than the external emulsification effect. The purity and stability of the product are improved.

[0025] When some inorganic materials are combined, the interface bonding is poor (such as CF and PPS), resulting in the problem of reduced material performance. Polyurethane has isocyanate (-NCO) groups that can react with (-OH, -COOH) to form chemical bonds, and polyurethane itself has good compatibility with polymer materials, which better solves the interface bonding between inorganic materials and polymer materials and improves the performance of materials.

[0026] The carbon fiber high temperature resistant sizing agent for the PPS thermoplastic composite matrix prepared by the preparation method of the present invention has a static contact angle with the carbon fiber of 15 to 21 degrees and a mass loss of 8 to 29% at 330°C. The interfacial shear strength (IFSS) between the sized carbon fiber and PPS reaches 40 to 50 MPa, which is 25 to 56% higher than the IFSS of the unsized carbon fiber (32 MPa).

[0027] The method of the present invention is characterized by high efficiency, environmental protection, and large-scale production. The prepared sizing agent can improve the interface bonding when inorganic materials are bonded, and can be used in the fields of aerospace, medical treatment, machinery, automobiles, rail transportation, oil transportation, etc. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0029] Example 1

[0030] A carbon fiber high temperature resistant sizing agent and a preparation method for a PPS thermoplastic composite material matrix, the steps are as follows:

[0031] (1) Under nitrogen atmosphere, at a reaction temperature of 75°C, 1 mol of diisocyanate is added to 1 mol of polyether diol or polyester diol for addition reaction, and the hydrogen of the alcohol hydroxyl group is added to the nitrogen atom of the isocyanate group. The reaction has no by-products. During the reaction, a small amount of diisocyanate is gradually added, and the amount added is 1% of the amount of diisocyanate added at the beginning of the reaction. The reaction time is 2 hours. After the reaction is completed, a group compound with active hydrogen is added to react with the terminal group -NCO for chain extension reaction, and a catalyst is added to catalyze the reaction. The reaction time is 3 hours to generate a PU prepolymer containing a hydrophilic structure;

[0032] (2) Determine the end group (-NCO) content of the polyurethane prepolymer. When it no longer changes, the reaction is complete. Add a neutralizer and water and disperse in water to form an aqueous polyurethane dispersion. Add 12 wt% acetone while stirring to reduce the polymer viscosity so that the aqueous polyurethane dispersion is evenly dispersed and react for 3 hours.

[0033] (3) Add 5% of a highly active polyamine chain extender to the polyurethane aqueous dispersion to carry out a chain extension reaction, thereby adjusting the ratio of soft and hard segments and the molecular weight in the polyurethane molecule to obtain a polyurethane dispersion with a higher relative molecular weight.

[0034] (4) Add 1% cross-linking agent and 0.5% wetting agent.

[0035] The static contact angle of the carbon fiber high temperature resistant sizing agent for the PPS thermoplastic composite matrix with the carbon fiber is 21°, and the mass loss at 330°C is 29%; the interface shear strength between the carbon fiber and PPS after sizing with this sizing agent is 40MPa.

[0036] Example 2

[0037] A carbon fiber high temperature resistant sizing agent for a PPS thermoplastic composite material matrix and a preparation method thereof, the steps are as follows:

[0038] (1) Under nitrogen atmosphere, reaction temperature is 72°C, 1 mol of diisocyanate is added to 1 mol of polyether diol or polyester diol for addition reaction, hydrogen of alcohol hydroxyl group is added to nitrogen atom of isocyanate group, and there is no by-product in the reaction. During the reaction, a small amount of diisocyanate is gradually added, and the amount added is 5% of the amount of diisocyanate added at the beginning of the reaction, and the reaction time is 2.5h. After the reaction is completed, a compound with active hydrogen group is added to react with terminal group -NCO for chain extension reaction, and a catalyst is added for catalytic reaction, and the reaction time is 3.5h to generate a PU prepolymer containing hydrophilic structure;

[0039] (2) Determine the end group (-NCO) content of the polyurethane prepolymer. When it no longer changes, the reaction is complete. Add a neutralizer and water and disperse in water to form an aqueous polyurethane dispersion. Add 15 wt% acetone while stirring to reduce the polymer viscosity so that the aqueous polyurethane dispersion is evenly dispersed and react for 3 hours.

[0040] (3) Adding 2% of a highly active polyamine chain extender to the polyurethane aqueous dispersion to carry out a chain extension reaction, thereby adjusting the ratio of soft and hard segments and the molecular weight in the polyurethane molecule to obtain a polyurethane dispersion with a higher relative molecular weight.

[0041] (4) Add 2% crosslinking agent and 1.5% wetting agent.

[0042] The static contact angle between the carbon fiber high temperature resistant sizing agent for the PPS thermoplastic composite matrix and the carbon fiber is 18°, and the mass loss at 330°C is 18%; the interface shear strength between the carbon fiber and PPS after sizing with this sizing agent is 45MPa.

[0043] Example 3

[0044] A carbon fiber high temperature resistant sizing agent for a PPS thermoplastic composite material matrix and a preparation method thereof, the steps are as follows:

[0045] (1) Under nitrogen atmosphere, at a reaction temperature of 70°C, 1 mol of diisocyanate is added to 1 mol of polyether diol or polyester diol for addition reaction, and the hydrogen of the alcohol hydroxyl group is added to the nitrogen atom of the isocyanate group. The reaction has no by-products. During the reaction, a small amount of diisocyanate is gradually added, and the amount added is 10% of the amount of diisocyanate added at the beginning of the reaction. The reaction time is 3 hours. After the reaction is completed, a group compound with active hydrogen is added to react with the terminal -NCO to undergo a chain extension reaction, and a catalyst is added to catalyze the reaction. The reaction time is 4 hours to generate a PU prepolymer containing a hydrophilic structure;

[0046] (2) Determine the end group (-NCO) content of the polyurethane prepolymer. When it no longer changes, the reaction is complete. Add a neutralizer and water and disperse in water to form an aqueous polyurethane dispersion. Add 10 wt% acetone while stirring to reduce the polymer viscosity so that the aqueous polyurethane dispersion is evenly dispersed and react for 3 hours.

[0047] (3) Add 6% of highly active polyamine chain extender to the polyurethane aqueous dispersion to carry out chain extension reaction, adjust the ratio of soft and hard segments and molecular weight in the polyurethane molecule, and obtain a polyurethane dispersion with a higher relative molecular weight.

[0048] (4) Add 4% cross-linking agent and 2% wetting agent.

[0049] The static contact angle between the carbon fiber high temperature resistant sizing agent for the PPS thermoplastic composite matrix and the carbon fiber is 15°, and the mass loss at 330°C is 8%; the interface shear strength between the carbon fiber and PPS after sizing with this sizing agent is 50MPa.

[0050] Example 4

[0051] A carbon fiber high temperature resistant sizing agent for a PPS thermoplastic composite material matrix and a preparation method thereof, the steps are as follows:

[0052] (1) Under nitrogen atmosphere, at a reaction temperature of 70°C, 1 mol of diisocyanate is added to 1 mol of polyether diol or polyester diol for addition reaction, and the hydrogen of the alcohol hydroxyl group is added to the nitrogen atom of the isocyanate group. The reaction has no by-products. During the reaction, a small amount of diisocyanate is gradually added, and the amount added is 8% of the amount of diisocyanate added at the beginning of the reaction. The reaction time is 3 hours. After the reaction is completed, a group compound with active hydrogen is added to react with the terminal -NCO to undergo a chain extension reaction, and a catalyst is added to catalyze the reaction. The reaction time is 3.5 hours to generate a PU prepolymer containing a hydrophilic structure;

[0053] (2) Determine the end group (-NCO) content of the polyurethane prepolymer. When it no longer changes, the reaction is complete. Add a neutralizer and water and disperse in water to form an aqueous polyurethane dispersion. Add 13 wt% acetone while stirring to reduce the polymer viscosity so that the aqueous polyurethane dispersion is evenly dispersed and react for 3 hours.

[0054] (3) Add 3% of highly active polyamine chain extender to the polyurethane aqueous dispersion to carry out chain extension reaction, adjust the ratio of soft and hard segments and molecular weight in the polyurethane molecule, and obtain a polyurethane dispersion with a higher relative molecular weight.

[0055] (4) Add 3% cross-linking agent and 0.8% wetting agent.

[0056] The static contact angle between the carbon fiber high temperature resistant sizing agent for the PPS thermoplastic composite matrix and the carbon fiber is 16°, and the mass loss at 330°C is 10%; the interface shear strength between the carbon fiber and PPS after sizing with this sizing agent is 49MPa.

[0057] Finally, it should be noted that the above is only a preferred embodiment of the present invention and does not limit it. Although this patent is described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions recorded in the aforementioned embodiments or to replace some of the technical features therein with equivalents. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention are included in the protection scope of the present invention.

Claims

1. A method for preparing a high temperature resistant sizing agent for carbon fiber based on a PPS thermoplastic composite material matrix, It is characterized in that The following steps are involved: (1) Prepolymerization stage: diisocyanate reacts with polyether diol or polyester diol to form a prepolymer terminated by isocyanate groups; hydrophilic groups are introduced into the polyurethane prepolymer terminated by isocyanate, and a catalyst is added to react to form a polyurethane prepolymer containing a hydrophilic structure; (2) Water dispersion formation stage: adding a neutralizing agent and water to disperse the polyurethane prepolymer containing a hydrophilic structure in water to form an aqueous polyurethane dispersion; (3) Chain extension reaction stage: adding highly active polyamine chain extenders to further extend the chains of the aqueous polyurethane dispersion in a dispersed state to obtain a polyurethane dispersion with a high relative molecular mass; (4) Cross-linking reaction stage: Add two types of additives, cross-linking agent and wetting agent, to start the cross-linking reaction and improve the temperature resistance and wettability of polyurethane.

2. The method for preparing a carbon fiber high temperature resistant sizing agent for a PPS thermoplastic composite material matrix according to claim 1, It is characterized in that In the prepolymerization stage, under a nitrogen atmosphere, an equivalent amount of diisocyanate is first added at the beginning of the reaction to react with the polyether diol or polyester diol, and a small amount of diisocyanate is gradually added during the reaction. The reaction temperature is 70-75°C and the reaction time is 2-3h. A small amount of diisocyanate is gradually added during the reaction, and the amount added is 1% to 10% of the amount of diisocyanate first added at the beginning of the reaction.

3. The method for preparing a high temperature resistant sizing agent for carbon fiber based on a PPS thermoplastic composite material matrix according to claim 1, It is characterized in that In the prepolymerization stage, the hydrophilic group refers to a group compound with active hydrogen, the catalyst is organic tin, organic bismuth or dibutyl dilauric acid, and the time for introducing the hydrophilic group and adding the catalyst to react is 3 to 4 hours.

4. The method for preparing a carbon fiber high temperature resistant sizing agent for a PPS thermoplastic composite material matrix according to claim 1, It is characterized in that During the stage of forming the aqueous dispersion, the isocyanate content of the polyurethane prepolymer terminal group is measured. If it no longer changes, it means that the reaction is complete.

5. The method for preparing a carbon fiber high temperature resistant sizing agent for a PPS thermoplastic composite material matrix according to claim 1, It is characterized in that In the stage of forming the water dispersion, when the polyurethane molecular chains are emulsified and dispersed in water, the self-emulsification step time should be ≤30 minutes, and the emulsification temperature should be ≤30°C.

6. The method for preparing a carbon fiber high temperature resistant sizing agent for a PPS thermoplastic composite material matrix according to claim 1, It is characterized in that In the stage of forming the aqueous dispersion, 10-15 wt% of an organic solvent may be added to reduce the viscosity of the polymer and apply shear force to facilitate uniform dispersion; wherein the organic solvent is any one of acetone, dimethylformamide (DMF) or N-methylpyrrolidone (NMP).

7. The method for preparing a carbon fiber high temperature resistant sizing agent for a PPS thermoplastic composite material matrix according to claim 1, It is characterized in that In the chain extension reaction stage, a highly active polyamine chain extender is added to adjust the ratio of soft and hard segments and the molecular weight in the polyurethane molecule, and the added amount is 2-6% of the mass of the polyurethane water dispersion.

8. The method for preparing a high temperature resistant sizing agent for carbon fiber based on a PPS thermoplastic composite material matrix according to claim 1, It is characterized in that In the cross-linking reaction stage, the cross-linking agent is any one of organic peroxides, silanes, acrylic acid, acrylamide, hydroxyethyl acrylate, divinylbenzene, diisocyanate, N,N-methylenebisacrylamide (MBA) or any combination thereof, and the added amount is 1 to 4% of the mass of the polyurethane aqueous dispersion.

9. The method for preparing a high temperature resistant sizing agent for carbon fiber based on a PPS thermoplastic composite material matrix according to claim 8, It is characterized in that In the cross-linking reaction stage, the cross-linking agent is CA-01, CA-02, Any one or any combination of CA-50 is added in an amount of 2 to 3% of the mass of the polyurethane aqueous dispersion.

10. The method for preparing a carbon fiber high temperature resistant sizing agent for a PPS thermoplastic composite material matrix according to claim 1, It is characterized in that In the cross-linking reaction stage, the wetting agent is any one of alkyl sulfates, sulfonates, fatty acids, carboxylic acid soaps, phosphates, polyoxyethylene alkylphenol ethers, polyoxyethylene fatty alcohol ethers, polyoxyethylene polyoxypropylene block copolymers or any combination thereof, and the added amount is 0.5-2% of the mass of the polyurethane aqueous dispersion.

11. The method for preparing a carbon fiber high temperature resistant sizing agent for a PPS thermoplastic composite material matrix according to claim 1, It is characterized in that In the cross-linking reaction stage, the wetting agent is FS-640, PSA-96, Twin245, TEGO Dispers 688 or any combination thereof, the addition amount is 0.8-1.5% of the mass of the polyurethane aqueous dispersion.

12. A sizing agent prepared by the method for preparing a carbon fiber high temperature resistant sizing agent for a PPS thermoplastic composite material matrix according to any one of claims 1 to 11, Its characteristics are: The static contact angle between the sizing agent and the carbon fiber is 15-21 degrees, and the mass loss at 330 degrees C is 8-29 percent; the interface shear strength (IFSS) between the sizing carbon fiber and PPS reaches 40-50 MPa.