Method for preparing Kepp seal coat by using steel slag

By simultaneously spraying fast cracking high solid content emulsified asphalt and steel slag to form a steel slag gravel seal, combined with a fog seal and basalt micro-surface, the low construction efficiency and poor bonding effect of the steel slag seal in the existing technology are solved. solve the problem, improve the wear resistance and water sealing performance of high-grade roads, and improve the resource utilization of steel slag.

CN118814554AInactive Publication Date: 2024-10-22SHANGHAI TUOPU ROAD MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411225392.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When the existing technology uses steel slag to prepare the sealing layer of high-grade roads, the construction efficiency is low and the bonding effect between steel slag and asphalt is poor, resulting in potential road safety hazards and low resource utilization.

Method used

Simultaneous spraying of fast cracking high solid content emulsified asphalt and steel slag is used to form a steel slag gravel seal, and a fog seal is sprayed on top of it. Finally, basalt is used as aggregate for micro-surfacing, which simplifies the process and improves the bonding effect. and water sealing performance.

Benefits of technology

It improves the wear resistance, water sealing ability and life of the road, enhances the bonding effect between steel slag and asphalt, shortens the construction time, is suitable for the construction of high-grade roads, and improves the utilization rate of steel slag.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118814554A_ABST
    Figure CN118814554A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a Kaipu seal coat by using steel slag, which comprises the following steps: 1) cleaning and blowing off sundries on a base layer, and repairing the base layer; (2) fast-breaking high-solid-content emulsified asphalt and steel slag are sprayed synchronously, the emulsified asphalt is ground after being subjected to primary demulsification, and a steel slag gravel sealing layer is formed after forming; the solid content of the high-solid-content emulsified asphalt is greater than or equal to 65%; (3) adsorbing pumice, spraying a fog sealing layer on the steel slag gravel sealing layer, and demulsifying and forming the fog sealing layer; and (3) micro-surfacing or slurry sealing is conducted on the steel slag and gravel sealing layer with graystone as aggregate, a composite surface wearing layer is formed, and the Kepu sealing layer is obtained after forming. The Kepp seal coat is prepared from the steel slag, the hardness and wear resistance of the steel slag are fully utilized, the wear resistance of the pavement is greatly improved, the water sealing coefficient is improved, and the service life of the road is prolonged; the steel slag resource is recycled, waste is turned into wealth, and huge economic benefits are created.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of highway maintenance, and in particular relates to a method for preparing a cape seal layer by using steel slag. Background Art

[0002] Steel slag is an industrial solid waste, which is produced in large quantities every year. If it is not treated, it will have an adverse impact on the environment. Although steel slag has a wide range of applications, its utilization rate in my country is still low. The rational use of steel slag to reuse resources can turn waste into treasure and create huge economic benefits. It is an effective way to achieve sustainable development and is of great significance to the country and society.

[0003] Chinese patent CN113250036A discloses a method for preparing asphalt synchronous crushed stone upper sealing layer using steel slag, which includes the following steps: the first step is pretreatment of the base layer; the second step is spraying the first layer of emulsified asphalt, rolling it flat, drying it, and spreading steel slag; the third step is spraying the second layer of emulsified asphalt, rolling it flat, and drying it. This patent adopts a variant asynchronous construction method, first spreading emulsified asphalt to break the emulsion, then spreading stones, and then spreading emulsified asphalt after the stones stick to it. The steps are relatively complicated, resulting in low construction efficiency, which leads to a long construction time; at the same time, because the process is not perfect after the emulsified asphalt is spread, the bonding effect between the stone and the asphalt is poor, and the bonding between the steel slag and the asphalt is insufficient. After opening the traffic, there may be a risk of stone falling off and scattering, which affects traffic and causes harm to vehicles. Therefore, it can only be used to make low-grade roads and cannot be used on high-grade roads.

[0004] The difference between low-grade and high-grade pavements in the highway industry is that high-grade roads refer to expressways and first-class roads, which generally have faster speeds and larger traffic volumes. Currently, the technology of directly using steel slag as raw material to prepare high-grade pavements has yet to be improved. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a Cape seal using steel slag, which uses steel slag to prepare a Cape seal, fully utilizes the hardness and wear resistance of the steel slag, greatly improves the wear resistance of the road surface, improves the water sealing coefficient, and increases the life of the road; reuses steel slag resources, turns waste into treasure, and creates huge economic benefits.

[0006] To achieve the above purpose, the technical solution of the present invention is as follows:

[0007] A method for preparing a cape seal using steel slag comprises the following steps:

[0008] 1) Clean and blow away the debris on the base layer and repair the base layer;

[0009] 2) Spraying fast-cracking high-solid emulsified asphalt and steel slag simultaneously, rolling the emulsified asphalt after initial demulsification, and forming a steel slag gravel seal after molding; the solid content of the high-solid emulsified asphalt is ≥65%;

[0010] 3) Adsorb pumice and spray a mist seal layer on the steel slag gravel seal layer, and the mist seal layer breaks the emulsion and takes shape;

[0011] 4) Using basalt as aggregate to perform micro-surfacing or slurry sealing on the steel slag crushed stone seal layer to form a composite surface wear layer, and obtaining a Cape seal layer after molding.

[0012] Preferably, the particle size of the steel slag is 3-10 mm, the crushing value is ≤26%, and the f-CaO content is ≤5%.

[0013] Preferably, the time taken for the initial demulsification of the emulsified asphalt is 5 to 15 minutes.

[0014] Preferably, the temperature of the emulsified asphalt is 40-60°C, preferably 55-60°C.

[0015] Preferably, the thickness of the steel slag crushed stone seal is 3 to 10 mm, preferably 3 mm, 5 mm or 9 mm.

[0016] Preferably, the amount of emulsified asphalt sprayed is 1.3-2.3 kg / m according to the thickness of the steel slag gravel seal. 2 Preferably, for steel slag thickness of 3mm, 5mm or 9mm, the amount of emulsified asphalt sprayed is 1.3-1.6kg / m 2 , 1.4~1.9kg / m 2 , 1.7~2.3kg / m 2 .

[0017] Preferably, the rolling time is 5 to 10 minutes.

[0018] Preferably, the spraying amount of the fog seal layer is 0.2-1.2 kg / m 2 , preferably 0.4kg / m 2 .

[0019] Preferably, the demulsification forming time of the mist seal layer is 0.5 to 1 hour.

[0020] The present invention uses steel slag to prepare a gravel seal, adds a fog seal to the steel slag gravel seal, and then uses basalt as an aggregate for micro-surfacing or a slurry seal to combine it. The prepared Cape seal increases the life of the pavement, increases the pavement's resistance to water damage, and improves the pavement's water-sealing capacity. It can be used on high-grade pavements, and will increase the application scope of steel slag, making the utilization rate of steel slag more sufficient.

[0021] The present invention uses steel slag to prepare steel slag chip seal, and simultaneously sprays fast-cracking high-solid emulsified asphalt, the solid content of the fast-cracking high-solid emulsified asphalt is ≥65%, thereby increasing the viscosity of the emulsified asphalt and greatly improving the emulsification speed of the emulsified asphalt. The use temperature of the emulsified asphalt is increased to 40-60°C, preferably 55-60°C, to improve the emulsification speed of the emulsified asphalt. During construction, a chip seal synchronous sealing vehicle is selected to realize synchronous and rapid spreading of the emulsified asphalt and steel slag.

[0022] There is no restriction on the source of the steel slag, which is preferably crushed converter drum steel slag with a particle size of 3 to 10 mm and an f-CaO content of ≤5wt%. By limiting the particle size of the steel slag, the strength of the steel slag particles meets the requirements of road construction. The f-CaO content refers to the free CaO content in the steel slag. The f-CaO content of the steel slag is limited to ≤5wt%, eliminating the instability of the steel slag, making its performance indicators meet the requirements of industry standards, and preventing the subsequent disintegration and pulverization of the steel slag from causing road surface bulges and cracks. In some embodiments of the present invention, the particle size of the steel slag is 3 to 10 mm, and the f-CaO content is ≤5%wt. In some embodiments of the present invention, the crushing value of the steel slag is further limited to ≤26%, thereby meeting the requirements of high-grade roads.

[0023] The thickness of the steel slag gravel seal is generally 3-10mm. According to the actual road conditions and steel slag conditions, the preferred thickness of the steel slag gravel seal is 3mm, 5mm, 9mm, etc. According to the thickness of the steel slag gravel seal, the amount of emulsified asphalt to be spread is 1.3-2.3kg / m 2 For the thickness of steel slag gravel seal layer of 3mm, 5mm and 9mm, the amount of emulsified asphalt sprayed is 1.3-1.6kg / m 2 , 1.4 -1.9kg / m 2 , 1.7-2.3kg / m 2 .

[0024] After the emulsified asphalt is initially demulsified, a rubber-wheel roller is introduced to compact it, which helps to arrange the steel slag, enhances the bonding between the steel slag and asphalt, increases the bonding effect between the steel slag gravel seal layer and the original road surface, and increases the durability of the steel slag gravel seal layer.

[0025] After the steel slag gravel seal is formed, spray the mist seal on the steel slag gravel seal to break the emulsion and form the mist seal. The introduction of the mist seal also increases the durability and water sealing performance of the steel slag gravel seal. The spraying amount of the mist seal is 0.2-1.2kg / m 2 , preferably 0.4kg / m 2 .

[0026] Finally, basalt is used as aggregate for micro-surfacing or slurry sealing on the surface of the fog seal layer. After spreading, the fog seal layer can be opened to traffic after demulsification and formation. The demulsification time is 0.5-1h. After the steel slag micro-surfacing is formed, it can be directly opened to traffic without rolling.

[0027] The original process of emulsified asphalt, steel slag, and emulsified asphalt step-by-step spreading and waiting was simplified to a fast process of emulsified asphalt / steel slag and fog seal. At the same time, fast-cracking high-solid emulsified asphalt and fog seal were selected to increase the demulsification speed, increase construction efficiency, and achieve the purpose of rapid opening of traffic.

[0028] Compared with the existing process, the invention has the following beneficial effects:

[0029] Using steel slag as aggregate for gravel seal can replace commonly used aggregates such as basalt. Since steel slag itself has a porous structure, it can be better combined with emulsified asphalt, thereby increasing the life of the road surface and recycling resources. A fog seal is introduced on the basis of the steel slag gravel seal, while increasing the durability and water sealing performance of the steel slag gravel seal. The prepared Cape seal structure increases the life of the road surface. The present invention simultaneously sprays fast-cracking high-solid emulsified asphalt and steel slag when preparing the steel slag gravel seal, which simplifies the process and shortens the time. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Schematic diagram of a flow chart of an embodiment of the present invention. DETAILED DESCRIPTION

[0031] The present invention will be further described below in conjunction with the embodiments and drawings.

[0032] Example 1

[0033] A method for preparing a cape seal using steel slag comprises the following steps:

[0034] 1) Clean and blow away the debris and soil on the road base, and cover the surface layers that need to be protected, such as curbstones and manhole covers, with plastic film;

[0035] 2) Spraying fast-cracking high-solid emulsified asphalt and steel slag simultaneously, after the emulsified asphalt is initially demulsified, rolling it with a rubber-wheel roller for 10 minutes, and forming a steel slag gravel seal layer after molding; the emulsified asphalt is prepared using the fast-cracking emulsifier Indulin AA-63D of Shanghai Invitrogen, with a solid content of 66% and a temperature of 60°C; the steel slag used is the converter drum slag of Shanghai Baosteel, with a particle size range of 8-10mm and an f-CaO content of no more than 5%;

[0036] 3) Adsorb pumice and spray a mist seal layer on the steel slag gravel seal layer. The mist seal layer will break up and take shape. The next step of construction will be carried out one week after the traffic is opened.

[0037] 4) For paving MS-III micro-surfacing, emulsified asphalt was used. The slow-cracking and fast-setting emulsifier Indulin MQ3 produced by Shanghai Invitrogen was used to prepare the emulsified asphalt. The steel slag used was from the converter drum slag of Shanghai Baosteel. The particle size range was: 0-9mm continuous graded steel slag, the f-CaO content did not exceed 5%, and the slag was opened to traffic after molding.

[0038] Example 2

[0039] The difference from Example 1 is that the next step of micro-surfacing construction is directly carried out after the mist seal layer is demulsified and formed.

[0040] Example 3

[0041] The difference from Example 1 is that the micro-surfacing uses the spreading micro-surfacing MS-II type micro-surfacing, and the steel slag used is from the converter drum slag of Shanghai Baosteel, with a particle size range of: 0-5mm continuous graded steel slag, and the fCaO content does not exceed 5%.

[0042] Comparative Example 1

[0043] The difference from Example 1 is that basalt with the same particle size is used instead of steel slag.

[0044] Comparative Example 2

[0045] The difference from Example 2 is that the micro-surfacing is directly spread without spreading the mist seal layer.

[0046] Comparative Example 3

[0047] The difference from Example 2 is that no micro-surfacing is applied after the mist seal layer is demulsified.

[0048] Table 1

[0049]

[0050] The construction time includes the time of each step, among which the time of covering and removing the plastic film is calculated as the same time. For the method of sweeping loss rate and gravel shedding rate, please refer to T / CECS G: M54-01-2023 Technical Specification for Highway Maintenance Gravel Seal. The water permeability coefficient indicates that the road surface has good water sealing performance. Wet wheel wear indicates good wear resistance and strong resistance to water damage.

[0051] The sweeping loss rate indicates the forming speed of the chip seal; the chip shedding rate indicates the bonding effect of the chip seal; the water permeability coefficient indicates the water sealing effect; and the wet wheel abrasion indicates the water damage resistance effect. The comparative examples and the results of the examples show that compared with the traditional basalt, the performance of steel slag can meet the pavement performance requirements and can replace basalt as road aggregate.

[0052] Comparative Example 1 shows that compared with traditional basalt, the performance of steel slag can meet the pavement performance requirements and can replace basalt as road aggregate. In addition, the introduction of steel slag has a smaller wet wheel wear data, which means that the road durability and water damage resistance are stronger. Comparing the wet wear, it is found that the wear resistance of steel slag is better than that of basalt, and the water damage resistance is stronger, so it can replace steel slag as road aggregate.

[0053] In Comparative Example 2, construction was carried out directly without spreading the mist seal layer, resulting in a high gravel loss rate, and pumice was easy to fall off. The loss rate by sweeping and brushing became larger, and pumice was easy to fly in the early stage. Construction could not be carried out until the gravel seal layer was completely compacted, which prolonged the construction time.

[0054] In Comparative Example 3, it is shown that if micro-surfacing is not added, the water damage resistance and wear resistance are poor, and there is a certain amount of water seepage, which shows that micro-surfacing brings good water sealing effect and water damage resistance effect.

Claims

1. A method for preparing a cape seal using steel slag, characterized in that: The steps include: 1) Clean and blow away the debris on the base layer and repair the base layer; 2) Spraying fast-cracking high-solid emulsified asphalt and steel slag simultaneously, rolling the emulsified asphalt after initial demulsification, and forming a steel slag gravel seal after molding; the solid content of the high-solid emulsified asphalt is ≥65%; 3) Adsorb pumice and spray a mist seal layer on the steel slag gravel seal layer, and the mist seal layer breaks the emulsion and takes shape; 4) Using basalt as aggregate to perform micro-surfacing or slurry sealing on the steel slag crushed stone seal layer to form a composite surface wear layer, and obtaining a Cape seal layer after molding.

2. The method for preparing a cape seal using steel slag as claimed in claim 1, characterized in that: The particle size of the steel slag is 3-10 mm, the crushing value is ≤26%, and the f-CaO content is ≤5%.

3. The method for preparing a cape seal using steel slag as claimed in claim 1, characterized in that: The temperature of the emulsified asphalt is 40-60°C, preferably 55-60°C.

4. The method for preparing a cape seal using steel slag as claimed in claim 1, characterized in that: The time required for the initial demulsification of emulsified asphalt is 5 to 15 minutes.

5. The method for preparing a cape seal using steel slag as claimed in claim 1, characterized in that: The thickness of the steel slag crushed stone seal layer is 3 to 10 mm, preferably 3 mm, 5 mm or 9 mm.

6. The method for preparing cape seal using steel slag as claimed in claim 1 or 5, characterized in that: According to the thickness of steel slag gravel seal, the amount of emulsified asphalt to be spread is 1.3-2.3kg / m 2 Preferably, for steel slag thickness of 3mm, 5mm or 9mm, the amount of emulsified asphalt sprayed is 1.3-1.6kg / m 2 , 1.4~1.9kg / m 2 , 1.7~2.3kg / m 2 .

7. The method for preparing a cape seal using steel slag as claimed in claim 1, characterized in that: The rolling time is 5 to 10 minutes.

8. The method for preparing a cape seal using steel slag as claimed in claim 1, characterized in that: The spraying amount of the fog seal layer is 0.2~1.2kg / m 2 , preferably 0.4kg / m 2 .

9. The method for preparing a cape seal using steel slag as claimed in claim 1, characterized in that: The demulsification and forming time of the fog seal layer is 0.5 to 2.0 hours.

Citation Information

Cited By

  • Preparation method of wet wheel abrasion test piece and experimental method based on wet wheel abrasion test piece

    CN119618767A