Preparation process and application of high-toughness fiber-reinforced recycled aggregate concrete

By pretreating concrete recycled aggregates and using expanded micropore anchoring micropowders and modified fibers, the problem of low mechanical properties of concrete recycled aggregates is solved, and its compressive strength and toughness are significantly improved, which is suitable for construction and other fields.

CN118908663APending Publication Date: 2024-11-08THE 4TH ENG CO LTD OF CHINA RAILWAY 16TH BUREAU GRP CO LTD +2
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411100978.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The mechanical properties of concrete recycled aggregates are low, mainly due to their high porosity and microcracks, which limit their wide application in construction and other fields.

Method used

By pretreating the regenerated aggregate, calcium bicarbonate is adsorbed and dihydrogen phosphate is loaded to form calcium dihydrogen phosphate solids to fill pores; at the same time, expandable micropore anchoring micropowders and modified fibers are used to enhance the mechanical strength of the concrete.

Benefits of technology

It effectively reduces the adverse effects of the porosity and mechanical properties of the regenerated aggregate, improves the compressive strength and toughness of concrete, enhances the bonding force between fiber and concrete matrix, and overcomes the problem of insufficient bonding force between fiber and concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908663A_ABST
    Figure CN118908663A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation process and application of high-toughness fiber-reinforced recycled aggregate concrete, and the preparation process comprises the following steps: (1) heating and leaching boric sludge with an acid solution, adding carbide slag, adding an alkali solution to adjust the system to be neutral or alkaline, standing, separating out a solid phase, calcining, grinding the obtained calcined product, and drying to obtain the high-toughness fiber-reinforced recycled aggregate concrete; the expansion type micropore anchoring micro powder is obtained. And (2) adding chopped organic fibers, a silane coupling agent and the expanded microporous anchoring micro-powder into absolute ethyl alcohol for reaction, then separating out the fibers, and airing the fibers to obtain the modified fibers. (3) taking the following raw materials: cement, composite coarse aggregate, river sand fine aggregate, the modified fiber, mineral powder and a water reducing agent; the composite coarse aggregate is formed by natural coarse aggregate and reinforced recycled coarse aggregate. The concrete material is obtained by uniformly mixing the raw materials with water. By treating the fibers and the recycled aggregate, the mechanical property of the concrete material prepared from the recycled aggregate is effectively overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete material preparation, and in particular to a preparation process and application of high-toughness fiber-reinforced recycled aggregate concrete. Background Art

[0002] Concrete materials are widely used due to their abundant sources, low prices, simple production processes, high compressive strength, good plasticity, and good durability. Moreover, with the development of social economy, the amount of concrete materials used is increasing. According to statistics, more than 4 billion tons of concrete will be produced globally in 2023. Buildings, roads, bridges, dams, embankments, etc. built with these concretes usually need to be demolished and rebuilt after reaching a certain period or being damaged. For example, my country stipulates that the service life benchmark period of concrete civil buildings is 50 years. After the concrete structure is demolished, a large amount of construction solid waste will be generated, most of which is landfilled and not effectively utilized. On the other hand, new concrete structures will consume a large amount of sand and gravel aggregates.

[0003] In order to realize the reuse of construction solid waste, people crush, screen, clean and grade the abandoned construction concrete blocks to form recycled aggregates, and then use these recycled aggregates to partially or completely replace natural aggregates to prepare new concrete materials, namely recycled aggregate concrete. This not only reduces the consumption of natural aggregates such as sand and gravel, saves resources, but also realizes the recycling of aggregates, which is conducive to the sustainable development of the construction industry. However, since the surface of recycled aggregates in concrete is rough, the water absorption rate is higher, and there are a large number of microcracks in them after crushing, the mechanical properties of recycled aggregate concrete are not as good as those of concrete prepared from sand and gravel natural aggregates under the same conditions, which limits the application of recycled aggregate concrete in some fields. Summary of the invention

[0004] In view of the above problems, the present invention provides a preparation process and application of high-toughness fiber-reinforced recycled aggregate concrete. The present invention effectively overcomes the mechanical properties of concrete materials prepared from recycled aggregates by processing fibers and recycled aggregates. Specifically, the technical solution of the present invention is as follows.

[0005] First, the present invention discloses a preparation process of high-toughness fiber-reinforced recycled aggregate concrete, comprising the following steps: (1) The boron mud is heated and leached with acid solution, and then carbide slag is first added, and then alkali solution is added to adjust the system to neutral or alkaline. After standing, the solid phase is separated and calcined, and then the calcined product is ground to obtain expandable microporous anchor powder for use.

[0006] (2) Adding short-cut organic fibers, a silane coupling agent and the expandable microporous anchoring powder into anhydrous ethanol, and keeping the mixture warm under heating and continuous stirring conditions, separating the short-cut organic fibers after completion, and drying them to obtain modified fibers for later use.

[0007] (3) The recycled coarse aggregate of concrete is immersed in a saturated solution of calcium bicarbonate. After the immersion, the coarse aggregate is separated, mixed with a saturated solution of dihydrogen phosphate, and then heated and evaporated to obtain reinforced recycled coarse aggregate for later use.

[0008] (4) Take the following raw materials in parts by weight: 60-80 parts of cement, 132-170 parts of composite coarse aggregate, 180-242 parts of river sand fine aggregate, 10-20 parts of the modified fiber, 5-18 parts of mineral powder, and 0.1-0.3 parts of water reducer. The composite coarse aggregate is formed by natural coarse aggregate and 40-60% of the reinforced recycled coarse aggregate. The above raw materials are mixed with water to obtain concrete material.

[0009] Furthermore, in step (1), the ratio of the borax mud to the acid solution is 1 g: 5-15 ml. Optionally, the mass fraction of the acid solution is 10-20%. The acid solution includes at least one of hydrochloric acid, sulfuric acid, nitric acid, etc.

[0010] Furthermore, in step (1), the heating leaching temperature is 40-50° C., and the leaching time is 2-3 hours, so as to leach the magnesium element in the boron mud.

[0011] Furthermore, in step (1), the mass ratio of the borax mud to the carbide slag is 1-1.4:0.6-0.75.

[0012] Furthermore, in step (1), the alkalinity is pH=8-12. Optionally, the alkaline solution includes at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate solution, and the like.

[0013] Furthermore, in step (1), the calcination treatment is carried out at a temperature of 830-950° C. and for a time of 30-50 min.

[0014] Furthermore, in step (1), the fineness of the expandable microporous anchoring powder is 200-400 mesh.

[0015] Furthermore, in step (2), the expandable microporous anchoring powder is 4-7% of the amount of chopped organic fiber, and the mass fraction of the silane coupling agent in the anhydrous ethanol is 0.5-1.1%. Optionally, the solid-liquid ratio of the chopped organic fiber, anchoring powder and ethanol is 1g:20-40ml.

[0016] Furthermore, in step (2), the short-cut organic fibers include any one of polyethylene fibers, polypropylene fibers, polyacrylonitrile fibers, polyvinyl alcohol fibers, etc. Optionally, the length of the short-cut organic fibers is 10-30 mm.

[0017] Furthermore, in step (2), the silane coupling agent includes any one of kh550, kh560, kh570, etc.

[0018] Furthermore, in step (2), the heating temperature is 40-60° C., and the insulation time is 20-35 min.

[0019] Furthermore, in step (3), the ratio of the recycled coarse aggregate to the saturated solution of calcium bicarbonate is 1 g: 15-30 ml. Optionally, the immersion time is 30-60 min, so that the saturated solution of calcium bicarbonate can penetrate into the recycled aggregate.

[0020] Furthermore, in step (3), the ratio of the coarse aggregate to the saturated solution of dihydrogen phosphate is 1 g: 3-5.5 ml. Optionally, the dihydrogen phosphate includes at least one of potassium dihydrogen phosphate, ammonium dihydrogen phosphate, sodium dihydrogen phosphate, etc.

[0021] Furthermore, in step (3), the evaporation temperature is 80-90°C.

[0022] Furthermore, in step (4), the water reducer includes any one of a polycarboxylate water reducer, a naphthalene-based water reducer, a lignin sulfonate water reducer, a melamine-based water reducer, an aminosulfonate water reducer, and the like.

[0023] Furthermore, in step (4), water is added according to a water-cement ratio of 0.4 to 0.45.

[0024] Secondly, the present invention discloses the application of the high-toughness fiber-reinforced recycled aggregate concrete obtained by the above-mentioned preparation process in the fields of construction, bridges, roads, water conservancy projects, marine engineering, etc.

[0025] Compared with the prior art, the technical solution of the present invention has at least the following beneficial effects: Concrete recycled aggregate has high porosity and internal microcracks when broken, which affects the mechanical strength of the prepared concrete. For this reason, the present invention pre-treats the concrete recycled aggregate, effectively reduces the porosity of the aggregate, thereby reducing the adverse effects on the mechanical properties of the concrete. Specifically, the present invention first adsorbs calcium bicarbonate in the recycled aggregate, and then loads excessive dihydrogen phosphate, and uses part of the dihydrogen phosphate to react with calcium bicarbonate to form a dihydrogen phosphate solid to compact and fill the pores in the recycled aggregate, thereby reducing the porosity of the recycled aggregate. At the same time, when the recycled aggregate enters the concrete, the product calcium hydroxide of the bicarbonate and cement hydration reaction reacts to form calcium carbonate, which can further play a role in filling and compacting the pores in the recycled aggregate, thereby reducing the porosity of the aggregate and reducing the adverse effects on the mechanical properties of the concrete.

[0026] In addition, the present invention further improves the mechanical strength of the prepared concrete by using high-toughness organic fibers. To this end, the present invention first uses acid solution to extract the boron mud to dissolve the magnesium ions therein, and then adds carbide slag, the hydroxide ions provided by which can neutralize the acid solution, and the calcium ions and the magnesium ions provided are converted into hydroxides under an alkaline environment and mixed with the boron mud. After subsequent calcination, the hydroxide is decomposed into calcium oxide and magnesium oxide and distributed in the matrix formed by the boron mud. At the same time, the decomposition of the hydroxide also forms a porous structure in the matrix, thereby obtaining an expanded microporous anchoring powder. The present invention further loads the expanded microporous anchoring powder onto the surface of the organic fiber through a coupling agent to form a modified fiber. When the modified fiber is added to the concrete, on the one hand, the good toughness of the organic fiber can effectively improve the mechanical strength of the concrete. On the other hand, after the moisture in the concrete enters the expanded microporous anchoring powder loaded on the fiber surface, the magnesium oxide therein reacts with the dihydrogen phosphate released by the recycled aggregate to form a hydration product struvite with high adhesion and high strength. At the same time, the porous structure of the anchoring powder makes it intertwined with the hydration and gelling products of cement, so that the fiber and the concrete matrix are more firmly bonded together, overcoming the insufficient bonding force between the organic fiber and the concrete matrix, and limiting the problem of improving the strength of concrete. On the other hand, the calcium oxide in the anchoring powder forms calcium hydroxide after meeting water to expand the volume of the anchoring powder particles, thereby forming several anchoring points on the fiber, further increasing the bonding force between the organic fiber and the concrete matrix, so that when the concrete is subjected to load and cracking, the fiber is more difficult to be extracted from the concrete, and the strength of the concrete structure is improved. In addition, in the process of preparing the expanded microporous anchoring powder, the mineral phase structure such as silicon tetrahedron in the boron mud matrix is ​​decomposed to form an active structure under the excitation of alkali solution and mechanical grinding, which can react with the hydration product of cement, calcium hydroxide, to form cementitious materials such as hydrated calcium silicate, which helps to improve the bonding force between fiber and concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] It should be noted that the drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention and do not constitute an improper limitation of the present invention.

[0028] Figure 1 This is a picture of the expandable microporous anchoring powder sample prepared in the following Example 1.

[0029] Figure 2 This is a graph showing the compressive strength test of the concrete material prepared in the following Example 1. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. Unless otherwise defined, all professional and scientific terms used in the present invention have the same meaning as those familiar to those skilled in the art. The preferred implementation methods and materials described in the present invention are only for demonstration purposes. The reagents or raw materials used in the present invention can be purchased through conventional channels. If there are no special instructions, the reagents or raw materials used in the present invention are used in a conventional manner in the art or are used according to the product specification. Now the technical scheme of the present invention is further described in conjunction with specific embodiments.

[0031] Example 1 A preparation process of high-tenacity fiber-reinforced recycled aggregate concrete comprises the following steps: (1) Mix the boron mud and 10% sulfuric acid at a ratio of 1g:15ml and stir evenly, then heat to 50℃ and keep warm for 2.5 hours. After completion, add carbide slag powder to the leaching system at a mass ratio of 1.2:0.7 for boron mud and carbide slag, stir for 5 minutes, then add sodium hydroxide solution to adjust the system to pH=11, then filter and separate the solid phase, heat it to 900℃ at a heating rate of 10℃ / min and keep warm for 40 minutes. Then cool to room temperature, grind the calcined product and pass it through a 300-mesh sieve to obtain the expandable microporous anchoring powder (such as Figure 1 as shown), for standby use.

[0032] (2) Add 20 mm long polypropylene fiber, silane coupling agent (kh550) and the expandable microporous anchor powder prepared in this example to anhydrous ethanol, wherein: the expandable microporous anchor powder accounts for 6% of the fiber mass, the mass fraction of the silane coupling agent in the anhydrous ethanol is 0.8%, and the solid-liquid ratio of the fiber, anchor powder and ethanol is 1g:35ml. Then heat to 50°C under continuous stirring and keep warm for 30 minutes. After completion, separate the fiber, dry it and obtain the modified fiber for standby use.

[0033] (3) Mix the recycled concrete coarse aggregate with a saturated solution of calcium bicarbonate at a ratio of 1 g:30 ml and soak for 50 minutes. After completion, filter and separate the coarse aggregate, mix it with a saturated solution of potassium dihydrogen phosphate at a ratio of 1 g:4.5 ml, and evaporate to dryness under stirring at a temperature of 80° C. to obtain reinforced recycled coarse aggregate. Mix the crushed stone natural coarse aggregate with 52% of the mass of the reinforced recycled coarse aggregate of this embodiment to obtain a composite coarse aggregate for use. The particle size distribution of the composite coarse aggregate is between 8 and 12 mm.

[0034] (4) Take the following raw materials in parts by weight: 72 parts of 42.5 ordinary Portland cement, 145 parts of the composite coarse aggregate of this embodiment, 220 parts of fine aggregate (river sand, particle size 0.2-0.8 mm), 14 parts of the modified fiber of this embodiment, 10 parts of mineral powder, and 0.25 parts of polycarboxylate water reducer. Mix the above raw materials with water at a water-cement ratio of 0.43 to obtain concrete material.

[0035] The concrete material prepared in this embodiment is poured into a mold to prepare a concrete specimen. Then, the compressive strength of the concrete specimen is tested according to the Standard for Test Methods for Physical and Mechanical Properties of Concrete (GB / T 50081-2019). Figure 2 The result is 61.43 MPa.

[0036] Example 2 A preparation process of high-tenacity fiber-reinforced recycled aggregate concrete comprises the following steps: (1) Mix the boron mud and 20% sulfuric acid at a ratio of 1g:5ml and stir evenly, then heat to 40℃ and keep warm for 3 hours. After completion, add carbide slag powder to the leaching system at a mass ratio of 1:0.6 between boron mud and carbide slag, stir for 5 minutes, then add sodium carbonate solution to adjust the system to pH=8, then filter and separate the solid phase, heat it to 950℃ at a heating rate of 10℃ / min and keep warm for 30 minutes. Then cool to room temperature, grind the calcined product and pass it through a 200-mesh sieve to obtain the expandable microporous anchor powder for later use.

[0037] (2) Add polyacrylonitrile fiber with a length of 10 mm, silane coupling agent (kh560) and the expandable microporous anchor powder prepared in this example to anhydrous ethanol, wherein: the expandable microporous anchor powder accounts for 4% of the fiber mass, the mass fraction of the silane coupling agent in the anhydrous ethanol is 0.5%, and the solid-liquid ratio of the fiber, anchor powder and ethanol is 1g:20ml. Then heat to 60°C under continuous stirring and keep warm for 20 minutes. After completion, separate the fiber, dry it and obtain the modified fiber for standby use.

[0038] (3) Mix the recycled concrete coarse aggregate with a saturated solution of calcium bicarbonate at a ratio of 1 g: 25 ml and soak for 30 minutes. After completion, filter and separate the coarse aggregate, mix it with a saturated solution of ammonium dihydrogen phosphate at a ratio of 1 g: 5.5 ml, and evaporate to dryness under stirring at a temperature of 90° C. to obtain reinforced recycled coarse aggregate. Mix the crushed stone natural coarse aggregate with 40% of the mass of the reinforced recycled coarse aggregate of this embodiment to obtain a composite coarse aggregate for use. The particle size distribution of the composite coarse aggregate is between 8 and 12 mm.

[0039] (4) Take the following raw materials in parts by weight: 80 parts of 42.5 ordinary Portland cement, 170 parts of the composite coarse aggregate of this embodiment, 242 parts of fine aggregate (river sand, particle size 0.2-0.8 mm), 20 parts of the modified fiber of this embodiment, 18 parts of mineral powder, and 0.3 parts of sodium lignin sulfonate water reducer. Mix the above raw materials with water at a water-cement ratio of 0.45 to obtain concrete material.

[0040] The concrete material prepared in this embodiment was poured into a mold to prepare a concrete specimen. The compressive strength of the concrete specimen was then tested according to the "Concrete Physical and Mechanical Properties Test Method Standard" (GB / T 50081-2019), and the result was 58.26 MPa.

[0041] Example 3 A preparation process of high-tenacity fiber-reinforced recycled aggregate concrete comprises the following steps: (1) Mix the boron mud and 15% nitric acid at a mass fraction of 1g:8ml and stir evenly, then heat to 40℃ and keep warm for 2 hours. After completion, add carbide slag powder to the leaching system at a mass ratio of 1.4:0.75 between boron mud and carbide slag, stir for 5 minutes, then add potassium hydroxide solution to adjust the system to pH=12, then filter and separate the solid phase, heat it to 830℃ at a heating rate of 10℃ / min and keep warm for 50 minutes. Then cool to room temperature, grind the calcined product and pass it through a 400-mesh sieve to obtain the expanded microporous anchor powder for later use.

[0042] (2) Add polyethylene fiber with a length of 30 mm, silane coupling agent (kh570) and the expandable microporous anchor powder prepared in this example to anhydrous ethanol, wherein: the expandable microporous anchor powder accounts for 7% of the fiber mass, the mass fraction of the silane coupling agent in the anhydrous ethanol is 1.1%, and the solid-liquid ratio of the fiber, anchor powder and ethanol is 1g:40ml. Then heat to 40°C under continuous stirring and keep warm for 35 minutes. After completion, separate the fiber, dry it and obtain the modified fiber for standby use.

[0043] (3) Mix the recycled concrete coarse aggregate with a saturated solution of calcium bicarbonate at a ratio of 1 g:15 ml and soak for 60 minutes. After completion, filter and separate the coarse aggregate, mix it with a saturated solution of sodium dihydrogen phosphate at a ratio of 1 g:3 ml, and evaporate to dryness under stirring at a temperature of 80°C to obtain reinforced recycled coarse aggregate. Mix the crushed stone natural coarse aggregate with 60% of the mass of the reinforced recycled coarse aggregate of this embodiment to obtain a composite coarse aggregate for use. The particle size distribution of the composite coarse aggregate is between 8 and 12 mm.

[0044] (4) Take the following raw materials in parts by weight: 60 parts of 42.5 ordinary Portland cement, 132 parts of the composite coarse aggregate of this embodiment, 180 parts of fine aggregate (river sand, particle size 0.2-0.8 mm), 10 parts of the modified fiber of this embodiment, 5 parts of mineral powder, and 0.1 parts of polycarboxylate water reducer. Mix the above raw materials with water at a water-cement ratio of 0.4 to obtain concrete material.

[0045] The concrete material prepared in this embodiment was poured into a mold to prepare a concrete specimen. The compressive strength of the concrete specimen was then tested according to the "Concrete Physical and Mechanical Properties Test Method Standard" (GB / T 50081-2019), and the result was 64.57 MPa.

[0046] Example 4 A preparation process of high-tenacity fiber-reinforced recycled aggregate concrete comprises the following steps: (1) The crushed stone natural coarse aggregate is mixed evenly with 52% by weight of recycled concrete coarse aggregate to obtain composite coarse aggregate for standby use. The particle size distribution of the composite coarse aggregate is between 8 and 12 mm.

[0047] (2) Take the following raw materials in parts by weight: 72 parts of 42.5 ordinary Portland cement, 145 parts of the composite coarse aggregate of this embodiment, 220 parts of fine aggregate (river sand, particle size 0.2-0.8 mm), 14 parts of the modified fiber prepared in the above embodiment 1, 10 parts of mineral powder, and 0.25 parts of polycarboxylate water reducer. Mix the above raw materials with water at a water-cement ratio of 0.43 to obtain concrete material.

[0048] The concrete material prepared in this embodiment was poured into a mold to prepare a concrete specimen. The compressive strength of the concrete specimen was then tested according to the "Concrete Physical and Mechanical Properties Test Method Standard" (GB / T 50081-2019), and the result was 55.18 MPa.

[0049] Example 5 A preparation process of high-tenacity fiber-reinforced recycled aggregate concrete comprises the following steps: Take the following raw materials in parts by weight: 80 parts of 42.5 ordinary Portland cement, 170 parts of the composite coarse aggregate of Example 2, 242 parts of fine aggregate (river sand, particle size 0.2-0.8 mm), 20 parts of polyacrylonitrile fiber with a length of 10 mm, 18 parts of mineral powder, and 0.3 parts of sodium lignin sulfonate water reducer. The above raw materials are mixed evenly with water at a water-cement ratio of 0.45 to obtain concrete material.

[0050] The concrete material prepared in this embodiment was poured into a mold to prepare a concrete specimen. The compressive strength of the concrete specimen was then tested according to the "Concrete Physical and Mechanical Properties Test Method Standard" (GB / T 50081-2019), and the result was 46.61 MPa.

[0051] Example 6 A preparation process of high-tenacity fiber-reinforced recycled aggregate concrete comprises the following steps: (1) Mix the boron mud and 20% sulfuric acid at a ratio of 1g:5ml and stir evenly, then heat to 40℃ and keep warm for 3 hours. Then add sodium carbonate solution to adjust the system to pH=8, then filter and separate the solid phase, heat it to 950℃ at a heating rate of 10℃ / min and keep warm for 30min. Then cool it to room temperature, grind the calcined product and pass it through a 200-mesh sieve to obtain microporous anchor powder for later use.

[0052] (2) Add polyacrylonitrile fiber with a length of 10 mm, silane coupling agent (kh560) and the microporous anchoring powder prepared in this example to anhydrous ethanol, wherein: the microporous anchoring powder accounts for 4% of the fiber mass, the mass fraction of the silane coupling agent in the anhydrous ethanol is 0.5%, and the solid-liquid ratio of the fiber, anchoring powder and ethanol is 1g:20ml. Then heat to 60°C under continuous stirring for 20 minutes. After completion, separate the fiber, dry it and obtain the modified fiber for standby use.

[0053] (3) Take the following raw materials in parts by weight: 80 parts of 42.5 ordinary Portland cement, 170 parts of the composite coarse aggregate of Example 2, 242 parts of fine aggregate (river sand, particle size 0.2-0.8 mm), 20 parts of the modified fiber of this example, 18 parts of mineral powder, and 0.3 parts of sodium lignin sulfonate water reducer. Mix the above raw materials with water at a water-cement ratio of 0.45 to obtain concrete material.

[0054] The concrete material prepared in this embodiment was poured into a mold to prepare a concrete specimen. The compressive strength of the concrete specimen was then tested according to the "Concrete Physical and Mechanical Properties Test Method Standard" (GB / T 50081-2019), and the result was 50.32 MPa.

[0055] Example 7 A preparation process of high-tenacity fiber-reinforced recycled aggregate concrete comprises the following steps: (1) Mix the boron mud and clean water at a ratio of 1g:8ml and stir evenly, then heat to 40℃ and keep warm for 2 hours. After completion, add carbide slag powder to the leaching system at a mass ratio of 1.4:0.75 for boron mud and carbide slag, stir for 5 minutes, then add nitric acid to adjust the system to pH=12, then filter and separate the solid phase, heat it to 830℃ at a heating rate of 10℃ / min and keep warm for 50 minutes. Then cool to room temperature, grind the calcined product and pass it through a 400-mesh sieve to obtain the expandable microporous anchor powder for later use.

[0056] (2) Add polyethylene fiber with a length of 30 mm, silane coupling agent (kh570) and the expandable microporous anchor powder prepared in this example to anhydrous ethanol, wherein: the expandable microporous anchor powder accounts for 7% of the fiber mass, the mass fraction of the silane coupling agent in the anhydrous ethanol is 1.1%, and the solid-liquid ratio of the fiber, anchor powder and ethanol is 1g:40ml. Then heat to 40°C under continuous stirring and keep warm for 35 minutes. After completion, separate the fiber, dry it and obtain the modified fiber for standby use.

[0057] (3) Take the following raw materials in parts by weight: 60 parts of 42.5 ordinary Portland cement, 132 parts of composite coarse aggregate of Example 3, 180 parts of fine aggregate (river sand, particle size 0.2-0.8 mm), 10 parts of the modified fiber of this example, 5 parts of mineral powder, and 0.1 parts of polycarboxylate water reducer. Mix the above raw materials with water at a water-cement ratio of 0.4 to obtain concrete material.

[0058] The concrete material prepared in this embodiment was poured into a mold to prepare a concrete specimen. The compressive strength of the concrete specimen was then tested according to the "Concrete Physical and Mechanical Properties Test Method Standard" (GB / T 50081-2019), and the result was 52.74 MPa.

[0059] Example 8 A preparation process of high-tenacity fiber-reinforced recycled aggregate concrete comprises the following steps: Take the following raw materials in parts by weight: 72 parts of 42.5 ordinary Portland cement, 145 parts of composite coarse aggregate of Example 1, 220 parts of fine aggregate (river sand, particle size 0.2-0.8 mm), 10 parts of mineral powder, and 0.25 parts of polycarboxylate water reducer. Mix the above raw materials and water at a water-cement ratio of 0.43 to obtain concrete material.

[0060] The concrete material prepared in this embodiment was poured into a mold to prepare a concrete specimen. The compressive strength of the concrete specimen was then tested according to the "Concrete Physical and Mechanical Properties Test Method Standard" (GB / T 50081-2019), and the result was 43.11 MPa.

[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art can still modify the technical solutions described in the above embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made shall be included in the protection scope of the present invention.

Claims

1. A preparation process of high-toughness fiber-reinforced recycled aggregate concrete, It is characterized in that The steps include: (1) The boron mud is heated and leached with acid solution, and then carbide slag is first added, and then alkali solution is added to adjust the system to neutral or alkaline, and after standing, the solid phase is separated and calcined, and then the calcined product is ground to obtain expandable microporous anchor powder for standby use; (2) adding chopped organic fibers, a silane coupling agent and the expandable microporous anchoring powder into anhydrous ethanol, and keeping the mixture warm under heating and continuous stirring conditions. After the chopped organic fibers are separated, the modified fibers are obtained after being dried and set aside. (3) placing the recycled coarse aggregate of concrete in a saturated solution of calcium bicarbonate and immersing it, separating the coarse aggregate after immersion, mixing it with a saturated solution of dihydrogen phosphate, and then heating and evaporating it to obtain reinforced recycled coarse aggregate for later use; (4) Take the following raw materials in parts by weight: 60-80 parts of cement, 132-170 parts of composite coarse aggregate, 180-242 parts of river sand fine aggregate, 10-20 parts of the modified fiber, 5-18 parts of mineral powder, and 0.1-0.3 parts of water reducer; wherein the composite coarse aggregate is formed by natural coarse aggregate and 40-60% of the reinforced recycled coarse aggregate; mix the above raw materials with water to obtain concrete material.

2. The preparation process of high-tenacity fiber-reinforced recycled aggregate concrete according to claim 1, It is characterized in that In step (1), the ratio of the boron mud to the acid solution is 1 g: 5-15 ml; Optionally, the mass fraction of the acid solution is 10-20%; Optionally, the acid solution includes at least one of hydrochloric acid, sulfuric acid, and nitric acid; Optionally, in step (1), the temperature of the heating extraction is 40-50° C., and the extraction time is 2-3 hours.

3. The preparation process of high-tenacity fiber-reinforced recycled aggregate concrete according to claim 1, It is characterized in that In step (1), the mass ratio of the borax mud to the carbide slag is 1-1.4:0.6-0.75; Optionally, in step (1), the alkalinity is pH=8-12; Optionally, in step (1), the alkali solution includes at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate solution.

4. The preparation process of high-tenacity fiber reinforced recycled aggregate concrete according to claim 1, It is characterized in that In step (1), the calcination temperature is 830-950°C and the calcination time is 30-50 min; Optionally, in step (1), the fineness of the expandable microporous anchoring powder is 200-400 mesh.

5. The preparation process of high-tenacity fiber-reinforced recycled aggregate concrete according to claim 1, It is characterized in that In step (2), the expandable microporous anchoring powder is 4-7% of the amount of chopped organic fibers, and the mass fraction of the silane coupling agent in the anhydrous ethanol is 0.5-1.1%; Optionally, in step (2), the solid-liquid ratio of the chopped organic fibers, anchoring powder and ethanol is 1g:20-40ml; Optionally, in step (2), the chopped organic fibers include any one of polyethylene fibers, polypropylene fibers, polyacrylonitrile fibers, and polyvinyl alcohol fibers; Optionally, in step (2), the length of the chopped organic fibers is 10 to 30 mm; Optionally, in step (2), the silane coupling agent includes any one of kh550, kh560, and kh570.

6. The preparation process of high-tenacity fiber-reinforced recycled aggregate concrete according to claim 1, It is characterized in that In step (2), the heating temperature is 40-60° C. and the insulation time is 20-35 min.

7. The preparation process of high-tenacity fiber-reinforced recycled aggregate concrete according to claim 1, It is characterized in that In step (3), the ratio of the recycled coarse aggregate of the concrete to the saturated solution of calcium bicarbonate is 1 g: 15-30 ml; optionally, in step (3), the immersion time is 30-60 min.

8. The preparation process of high-tenacity fiber-reinforced recycled aggregate concrete according to claim 1, It is characterized in that In step (3), the ratio of the coarse aggregate to the saturated solution of dihydrogen phosphate is 1g:3-5.5ml; Optionally, in step (3), the dihydrogen phosphate includes at least one of potassium dihydrogen phosphate, ammonium dihydrogen phosphate, and sodium dihydrogen phosphate; Furthermore, in step (3), the evaporation temperature is 80-90°C.

9. The process for preparing high-tenacity fiber-reinforced recycled aggregate concrete according to any one of claims 1 to 8, It is characterized in that In step (4), water is added according to a water-cement ratio of 0.4 to 0.45; Optionally, in step (4), the water reducer includes any one of a polycarboxylate water reducer, a naphthalene-based water reducer, a lignin sulfonate water reducer, a melamine-based water reducer, and an aminosulfonate water reducer.

10. Application of high-tenacity fiber-reinforced recycled aggregate concrete obtained by the preparation process according to any one of claims 1 to 9 in buildings, bridges, roads, water conservancy projects, and marine projects.

Citation Information

Cited By

  • Modified recycled coarse aggregate, preparation method thereof and high-performance fiber reinforced concrete

    CN120004528A

  • Preparation process of carbon reduction type lightweight high-strength aggregate concrete material

    CN120247500A

  • Preparation process of carbon-reducing lightweight high-strength aggregate concrete material

    CN120247500B