Composite TCO thin films, heterojunction solar cells and photovoltaic modules

By designing a composite TCO thin film structure, the problem of TCO thin films being unable to balance light transmittance and conductivity was solved, thus improving the performance of heterojunction solar cells.

CN118825091BActive Publication Date: 2026-11-10BYD CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311288723.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-28
Publication Date
2026-11-10
Estimated Expiration
2043-09-28

AI Technical Summary

Technical Problem

Existing silicon-based heterojunction solar cells' TCO thin films struggle to balance excellent light transmittance and conductivity, resulting in low short-circuit current density.

Method used

A composite TCO thin film structure is adopted, including a first TCO layer, a second TCO layer and a hybrid layer. The hybrid layer consists of alternating conductive and antireflective regions. Excellent light transmittance and conductivity are achieved by adjusting the material and thickness of each layer.

Benefits of technology

This improved the short-circuit current density and fill factor of heterojunction solar cells, thereby enhancing conversion efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825091B_ABST
    Figure CN118825091B_ABST
Patent Text Reader

Abstract

This invention relates to the field of solar cell technology, and discloses a composite TCO thin film, a heterojunction solar cell, and a photovoltaic module. The composite TCO thin film comprises a first TCO layer, a second TCO layer, and a hybrid layer stacked sequentially; wherein the hybrid layer includes multiple conductive regions and multiple anti-reflection regions, and both the conductive regions and the anti-reflection regions are in contact with the second TCO layer, with the conductive regions and the anti-reflection regions arranged alternately. The composite TCO thin film provided by this invention possesses both excellent light transmittance and conductivity, with a light transmittance of not less than 90% in the 400-1100nm wavelength range, and simultaneously exhibits (2.3-3)×10⁻⁶... ‑4 The low resistivity of Ω·cm enables heterojunction solar cells using this composite TCO thin film to have higher short-circuit current density and fill factor, resulting in higher conversion efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solar cell technology, specifically to composite TCO thin films, heterojunction solar cells, and photovoltaic modules. Background Technology

[0002] Silicon-based heterojunction solar cells (HJTs) have simple technology, low energy consumption, and high conversion efficiency. They have unique advantages in bifacial power generation and ultra-thin cells, making them an important direction for the future development of solar cells.

[0003] A typical HJT structure uses an N-type monocrystalline silicon wafer as a substrate. An intrinsic amorphous silicon layer and a doped N-type microcrystalline silicon layer are sequentially deposited on one side of the wafer. On the other side, an intrinsic amorphous silicon layer and a doped P-type microcrystalline silicon layer are sequentially deposited. Transparent conductive oxide (TCO) films are then deposited on the surfaces of the N-type and P-type microcrystalline silicon layers, respectively. Finally, double-sided metal electrodes are formed on the top layers on both sides using screen printing. Because the emitter conductivity of an HJT cell is poor, collecting current solely through metal grid lines is insufficient. Therefore, a TCO film that is both conductive and transparent is needed to transport charge. This requires the TCO film to possess both good optical and electrical properties.

[0004] CN114914311A discloses a conductive layer comprising, from the emitter upwards, a first TCO layer, a second TCO layer, a third TCO layer, and a fourth TCO layer. The first TCO layer has a thickness of 2-6 nm and is used to collect amorphous silicon current; the second TCO layer has a thickness of 4-10 nm and serves as a transition layer; the third TCO layer has a thickness of 80-100 nm and allows light transmission; and the fourth TCO layer has a thickness of 5-10 nm and is used to match the metal electrode. This technical solution only considers improving the electrical matching between the TCO film and the metal electrode and amorphous silicon, but neglects the fact that the excessively high conductivity of the outer film hinders visible light transmission, resulting in a lower short-circuit current density and negatively impacting battery performance.

[0005] Therefore, providing an improved TCO film that better balances light transmittance and conductivity is of great significance for improving the performance of HJT. Summary of the Invention

[0006] This invention addresses the problem that existing silicon-based heterojunction solar cells' TCO thin films struggle to achieve both excellent light transmittance and conductivity, resulting in low short-circuit current density. It provides composite TCO thin films, heterojunction solar cells, and photovoltaic modules.

[0007] To achieve the above objectives, the first aspect of the present invention provides a composite TCO film, the composite TCO film comprising a first TCO layer, a second TCO layer and a mixed layer stacked sequentially;

[0008] The hybrid layer includes multiple conductive regions and multiple antireflection regions, and both the conductive regions and the antireflection regions are in contact with the second TCO layer, with the conductive regions and the antireflection regions arranged alternately.

[0009] A second aspect of the present invention provides a heterojunction solar cell, the heterojunction solar cell comprising: an N-type monocrystalline silicon substrate, a first intrinsic amorphous silicon layer, a P-type microcrystalline silicon layer, a first conductive layer and a first metal electrode disposed sequentially from near to far on the front side of the substrate, and a second intrinsic amorphous silicon layer, an N-type microcrystalline silicon layer, a second conductive layer and a second metal electrode disposed sequentially from near to far on the back side of the substrate;

[0010] Wherein, the first conductive layer is the composite TCO thin film described in the first aspect above, and the first metal electrode contacts and covers the conductive area in the composite TCO thin film.

[0011] A third aspect of the present invention provides a photovoltaic module, including the heterojunction solar cell described in the second aspect above.

[0012] Through the above technical solution, the composite TCO thin film provided by the present invention has a multilayer film structure comprising a first TCO layer, a second TCO layer, and a hybrid layer. The hybrid layer includes multiple conductive regions and multiple antireflective regions, and both the conductive regions and the antireflective regions are in contact with the second TCO layer. The conductive regions and the antireflective regions are arranged alternately. Using the above-mentioned specific multilayer film structure, the TCO thin film can achieve a light transmittance of not less than 90% in the 400-1100nm wavelength range, while its resistivity is only (2.3-3)×10⁻⁶. -4 The composite TCO thin film achieves a balance between excellent light transmittance and conductivity, resulting in heterojunction solar cells with higher short-circuit current density and fill factor, and thus higher conversion efficiency. Attached Figure Description

[0013] Figure 1 This is a schematic diagram of the layer structure of the TCO thin film provided by the present invention.

[0014] Figure 2 This is a schematic diagram of the layer structure of the heterojunction solar cell provided by the present invention.

[0015] Figure 3 This is a front (top view) schematic diagram of the heterojunction solar cell provided by the present invention.

[0016] Explanation of reference numerals in the attached figures

[0017] 1. First TCO layer; 2. Second TCO layer; 3. Hybrid layer

[0018] 4. Conductive region; 5. Anti-reflection region; 101. N-type single-crystal silicon wafer substrate.

[0019] 102. First intrinsic amorphous silicon layer; 103. P-type microcrystalline silicon layer; 104. First conductive layer

[0020] 105. First metal electrode; 106. Second intrinsic amorphous silicon layer; 107. N-type microcrystalline silicon layer

[0021] 108. Second conductive layer; 109. Second metal electrode Detailed Implementation

[0022] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0023] The first aspect of this invention provides a composite TCO thin film, such as Figure 1 As shown, the composite TCO film includes a first TCO layer 1, a second TCO layer 2, and a mixed layer 3 stacked sequentially.

[0024] The hybrid layer 3 includes multiple conductive regions 4 and multiple antireflection regions 5, and both the conductive regions 4 and the antireflection regions 5 are in contact with the second TCO layer 2. The conductive regions 4 and the antireflection regions 5 are arranged alternately.

[0025] In this invention, TCO thin film refers to transparent conductive oxide thin film, which has characteristics such as high transmittance in the visible spectrum, wide bandgap, and low resistivity, and is widely used in the field of solar cells. The inventors of this invention have discovered that designing the TCO thin film as a composite structure having a first TCO layer, a second TCO layer, and a specific hybrid layer, wherein the hybrid layer is divided into different functional regions, specifically, the functional regions include multiple conductive regions and multiple anti-reflection regions, and both the conductive regions and the anti-reflection regions are in contact with the second TCO layer. The conductive regions and the anti-reflection regions are arranged alternately, which enables the TCO thin film to have excellent optical and conductive properties, exhibiting high light transmittance in the 400-1100nm wavelength range and high electrical conductivity, thereby improving the performance of heterojunction solar cells and increasing the short-circuit current density of heterojunction solar cells.

[0026] According to the present invention, the alternating arrangement of the conductive region 4 and the antireflection region 5 means that in the hybrid layer 3, the multiple conductive regions 4 do not contact each other, and each independently contacts the adjacent antireflection region 5 and the second TCO layer 2, and the end of each conductive region 4 facing away from the second TCO layer 2 is not completely covered by the antireflection region 5.

[0027] In this invention, the number of the plurality of conductive regions 4 and antireflection regions 5 in the hybrid layer 3 is relatively lenient, as long as the number of conductive regions 4 is consistent with the number of metal electrodes in the heterojunction solar cell, and the number of antireflection regions 5 is sufficient to achieve an alternating arrangement of the antireflection regions 5 and conductive regions 4 (in this invention, Figure 1 , Figure 2 and Figure 3 The number of conductive regions 4 and anti-reflection regions 5 shown is only for illustrating their alternating arrangement. Preferably, the number of conductive regions 4 (denoted as n) is ≥ 8 (n is an integer), and more preferably 8 ≤ n ≤ 20.

[0028] According to the present invention, when both ends of the hybrid layer 3 (in the direction in which the conductive region 4 and the antireflective region 5 are alternately arranged) are both conductive regions 4, the number of conductive regions 4 in the hybrid layer 3 is n, and the number of antireflective regions 5 is n-1. Preferably, n≥8 (n is an integer), and more preferably 8≤n≤20.

[0029] According to the present invention, when both ends of the hybrid layer 3 (in the direction in which the conductive region 4 and the antireflection region 5 are alternately arranged) are both antireflection regions 5, the number of conductive regions 4 in the hybrid layer 3 is n, and the number of antireflection regions 5 is n+1. Preferably, n≥8 (n is an integer), and more preferably 8≤n≤20.

[0030] According to the present invention, when the two ends of the hybrid layer 3 (in the direction in which the conductive region 4 and the antireflection region 5 are alternately arranged) are the conductive region 4 and the antireflection region 5 respectively, the number of both the conductive region 4 and the antireflection region 5 in the hybrid layer 3 is n. Preferably, n ≥ 8 (n is an integer), and more preferably 8 ≤ n ≤ 20.

[0031] According to the present invention, in the composite TCO thin film, the first TCO layer 1 has a high carrier concentration and excellent conductivity, mainly serving to collect current; the second TCO layer 2 mainly serves to conduct electricity and transmit light, and also has an anti-reflection effect, thus acting as an anti-reflection film; the hybrid layer 3 includes a conductive region 4 and an anti-reflection region 5, the conductive region 4 and the anti-reflection region 5 are in contact with each other, and are not distributed in an upper and lower layer positional relationship, but rather both are in contact with the second TCO layer 2; wherein, the anti-reflection region 5 mainly serves to reduce reflection, and since the anti-reflection region 5 is in contact with the second TCO layer 2, it can form a "double-layer anti-reflection film" with the second TCO layer 2, thereby significantly reducing light reflection in the visible light band, making the composite TCO thin film have better light transmittance; the conductive region 4 has a high carrier concentration and excellent conductivity, and since the conductive region 4 is in contact with the second TCO layer 2 and is not covered by the anti-reflection region 5, it can efficiently conduct current from the second TCO layer.

[0032] According to the present invention, in the composite TCO thin film, the material of the antireflection region 5 can be selected from MgF2, SiN... x At least one of SiO2, Al2O3, TiO2, and ZnS can effectively reduce the reflectivity of incident light on the silicon wafer surface, thus facilitating incident light absorption. Preferably, the antireflection region 5 is made of MgF2, SiN2, or SiN2. x At least one of SiO2.

[0033] According to the present invention, in the composite TCO film, the materials of the first TCO layer 1, the second TCO layer 2 and the conductive region 4 are each independently selected from at least one of IWO, ITO, AZO, ICO and VTTO.

[0034] In this invention, IWO refers to WO3-doped In2O3 material (In2O3 mass fraction not less than 90%); ITO refers to SnO2-doped In2O3 material (In2O3 mass fraction not less than 90%); AZO refers to Al2O3-doped ZnO material (ZnO mass fraction not less than 98%); ICO refers to CeO2-doped InO3 material (In2O3 mass fraction not less than 90%); VTTO refers to In2O3 material doped with various rare earth elements and metal oxides (In2O3 mass fraction not less than 99%, purchased from Pioneer Thin Film Materials Co., Ltd.).

[0035] According to the present invention, in the multilayer film structure of the composite TCO thin film, the first TCO layer 1, the second TCO layer 2, and the conductive region 4 can be made of the same material or different materials, and the present invention does not impose any particular limitation on this. From the perspective of improving the adaptability of the thin film interface, it is preferable that the first TCO layer 1, the second TCO layer 2, and the conductive region 4 are made of the same material.

[0036] In a preferred embodiment of the present invention, the first TCO layer 1, the second TCO layer 2 and the conductive region 4 are all made of ICO, which can bring high carrier mobility and low ICO / pa-Si:H interface contact resistance.

[0037] In this invention, IWO, ITO, AZO, ICO, and VTTO are transparent conductive film materials known in the art, and can all be understood according to the definitions known in the art.

[0038] According to the present invention, in the composite TCO film, by adjusting the contact area between the conductive region 4 and the second TCO layer 2, and the contact area between the antireflection region 5 and the second TCO layer 2, the composite TCO film can better balance excellent light transmittance and conductivity. Preferably, the ratio of the contact area between the conductive region 4 and the second TCO layer 2 to the contact area between the antireflection region 5 and the second TCO layer 2 is (0.02-0.03):1.

[0039] According to the present invention, in the composite TCO thin film, the thickness of the first TCO layer 1 is 2-10 nm, preferably 4-6 nm. The thickness of the first TCO layer 1 falling within the above range ensures both carrier collection efficiency and light transmittance.

[0040] According to the present invention, in the composite TCO thin film, the thickness of the second TCO layer 2 is 70-110 nm, preferably 80-100 nm. The thickness of the second TCO layer 2 falling within the above range can result in better photoelectric performance and better formation of a "double-layer antireflection film" with the antireflection region in the hybrid layer.

[0041] According to the present invention, in the composite TCO thin film, the thickness of the mixed layer 3 is 80-150 nm, preferably 100-120 nm. The thickness of the mixed layer 3 falling within the above range allows for better conductivity, thereby better guiding charge carriers into the metal electrode.

[0042] According to the present invention, in the composite TCO film, the first TCO layer 1, the second TCO layer 2 and the mixed layer 3, while satisfying the above-mentioned thickness range, preferably have a thickness ratio of the first TCO layer 1 to the second TCO layer 2 of 1:(7-40), which allows the composite TCO film to better balance excellent light transmittance and conductivity.

[0043] According to the present invention, the composite TCO film has excellent light transmittance and high light transmittance. In light transmittance testing, the composite TCO film exhibits a light transmittance of not less than 90% in the 400-1100 nm wavelength range.

[0044] In this invention, light transmittance is determined according to the method specified in GB / T 30983-2014.

[0045] According to the present invention, the composite TCO film exhibits excellent electrical conductivity. The resistivity of the composite TCO film is (2.3-3)×10⁻⁶. -4 Ω·cm.

[0046] In this invention, resistivity is measured according to the method specified in GB / T 4326-2006.

[0047] According to the present invention, the composite TCO thin film can be obtained by layer-by-layer deposition on a substrate using a target material. The target material used to deposit the first TCO layer 1, the second TCO layer 2, and the conductive region 4 can be selected from at least one of IWO, ITO, AZO, ICO, and VTTO; the target material used to deposit the antireflection region 5 can be selected from MgF2 and SiN. x The film is selected from at least one of SiO2, Al2O3, TiO2, and ZnS. The deposition coating can be prepared using conventional deposition coating processes and parameters in the art, including but not limited to magnetron sputtering, electron beam evaporation, and reactive plasma deposition.

[0048] According to a preferred embodiment of the present invention, the preparation process of the composite TCO thin film includes: firstly, depositing a first TCO layer 1 on a substrate, wherein the deposition conditions include: the introduced gas is a mixture of high-purity argon and high-purity hydrogen, the partial pressure of high-purity hydrogen is 0.4-1%, the target power is 2-2.5 kW, and the deposition temperature is 170-190°C; then, depositing a second TCO layer 2 on the surface of the first TCO layer 1, wherein the deposition conditions include: the introduced gas is a mixture of high-purity argon, high-purity hydrogen, and high-purity oxygen, the partial pressure of high-purity hydrogen is 0.5-1.5%, the partial pressure of high-purity oxygen is 3-10%, the target power is 2-2.5 kW, and the deposition temperature is 170-190°C; then, setting a mask above the second TCO layer 2 (the mask opening...). The conductive region 4 is deposited on the surface of the second TCO layer 2 through a mask, with the following deposition conditions: the gas introduced is a mixture of high-purity argon and high-purity hydrogen, the partial pressure of high-purity hydrogen is 1-1.5%, the target power is 2-2.5kW, and the coating temperature is 170-190℃; finally, the anti-reflection region 5 is deposited in the space on the surface of the second TCO layer 2 excluding the conductive region 4, and the conductive region 4 and the anti-reflection region 5 together form the mixed layer 3. For the deposition of the anti-reflection region 5, when the material of the anti-reflection region 5 is MgF2, polycrystalline granular raw material is used, and the thermal resistance method is used for evaporation, with a resistance current of 85-90A, and stable evaporation is performed after pre-melting; when the material of the anti-reflection region 5 is SiN... x When the antireflection zone 5 is made of SiO2, Al2O3, TiO2, or ZnS, a radio frequency (13.56MHz) magnetron sputtering method is used. The gas introduced is a mixture of high-purity SiH4 and high-purity NH3, with a volume ratio of NH3 / SiH4 of (3-4):1. The target power is 17-21kW, and the deposition temperature is 200℃. When the antireflection zone 5 is made of SiO2, Al2O3, TiO2, or ZnS, a radio frequency (13.56MHz) magnetron sputtering method is used. The introduced gas is high-purity argon (partial pressure percentage 90-99.9%) and high-purity oxygen (partial pressure percentage 0.1-10%). The target power is 1-5kW, and the deposition temperature is 150-200℃. After depositing the mixed layer 3, it is preferable to anneal the resulting composite film at 150-190℃ to improve the overall crystallinity of the film.

[0049] A second aspect of the present invention provides a heterojunction solar cell, such as... Figure 2 and Figure 3As shown, the heterojunction solar cell includes: an N-type monocrystalline silicon substrate 101, a first intrinsic amorphous silicon layer 102, a P-type microcrystalline silicon layer 103, a first conductive layer 104 and a first metal electrode 105 arranged sequentially from near to far on the front side of the substrate 101, and a second intrinsic amorphous silicon layer 106, an N-type microcrystalline silicon layer 107, a second conductive layer 108 and a second metal electrode 109 arranged sequentially from near to far on the back side of the substrate 101;

[0050] Wherein, the first conductive layer 104 is the composite TCO thin film described in the first aspect above, and the first metal electrode 105 contacts and covers the conductive region 4 in the composite TCO thin film.

[0051] In this invention, the specifications and materials of the N-type monocrystalline silicon substrate 101, the first intrinsic amorphous silicon layer 102, the P-type microcrystalline silicon layer 103, the first metal electrode 105, the second intrinsic amorphous silicon layer 106, the N-type microcrystalline silicon layer 107, the second conductive layer 108, and the second metal electrode 109 in the heterojunction solar cell are not particularly limited, and conventional choices in the art can be adopted.

[0052] According to the present invention, in the heterojunction solar cell, preferably, the upper surface of the conductive region 4 in the first conductive layer 104 completely overlaps with the lower surface of the first metal electrode 105, which facilitates better longitudinal transport of charge carriers to the metal electrode.

[0053] In this invention, the P-type microcrystalline silicon layer refers to a silicon layer doped with P-type and having a crystallinity of 40% or more, and the N-type microcrystalline silicon layer refers to a silicon layer doped with N-type and having a crystallinity of 40% or more, which can be understood according to the definitions known in the art.

[0054] The heterojunction solar cell provided by this invention contains a first conductive layer made of a specific composite TCO film of this invention. This composite TCO film can balance excellent light transmittance and conductivity. Compared with heterojunction solar cell products that use conventional TCO films for the first conductive layer, the heterojunction solar cell provided by this invention has a higher short-circuit current density and fill factor, and a higher conversion efficiency.

[0055] A third aspect of the present invention provides a photovoltaic module, including the heterojunction solar cell described in the second aspect above.

[0056] The present invention will be described in detail below through embodiments. In the following embodiments and comparative examples,

[0057] Unless otherwise specified, all materials used are common commercially available products.

[0058] Example 1

[0059] Preparation of TCO thin films:

[0060] i) Take a clean, smooth glass sheet (75mm × 25mm in size, 1mm in thickness) and place it in the coating machine. Use magnetron sputtering to deposit an ICO (1% by weight CeO2 + 99% by weight In2O3) thin film on the surface of the glass sheet (the gas introduced is a mixture of high-purity argon and high-purity hydrogen, with a partial pressure of 0.4% for high-purity hydrogen, a target power of 2.5KW, and a coating temperature of 180℃) to form the first TCO layer.

[0061] ii) Deposit an ICO (1% by weight CeO2 + 99% by weight In2O3) thin film on the surface of the first TCO layer (the gas introduced is a mixture of high-purity argon, high-purity hydrogen and high-purity oxygen, with the partial pressure of high-purity hydrogen accounting for 1%, the partial pressure of high-purity oxygen gradually increasing from 3% to 10%, the target power is 2.5KW, and the coating temperature is 180℃) to form a second TCO layer;

[0062] iii) A mask is placed above the second TCO layer (the openings of the mask correspond to the deposition positions of the conductive areas), and an ICO (1% by weight CeO2 + 99% by weight In2O3) thin film is deposited on the surface of the second TCO layer through the mask (the gas introduced is a mixture of high-purity argon and high-purity hydrogen, the partial pressure of high-purity hydrogen is 1%, the target power is 2.5KW, and the deposition temperature is 180℃) to form a conductive area; then, a MgF2 thin film is deposited in the space on the surface of the second TCO layer other than the conductive area (using polycrystalline granular raw materials, evaporation by thermal resistance method, slowly adjusting the evaporation current to 90A, pre-melting and then evaporating smoothly) to form an anti-reflection area. The conductive area and the anti-reflection area together form a hybrid layer.

[0063] The resulting composite film was annealed at 190℃ for 30 min to obtain a composite TCO film (denoted as P1).

[0064] In P1, the thickness of the first TCO layer is 4 nm, the thickness of the second TCO layer is 80 nm, and the thickness of the hybrid layer is 110 nm; the thickness ratio of the first TCO layer to the second TCO layer is 1:20; the ratio of the contact area between the conductive region and the second TCO layer and the contact area between the antireflection region and the second TCO layer is 0.028:1.

[0065] Fabrication of heterojunction solar cells:

[0066] 1) Texturing and cleaning the N-type single-crystal silicon wafer (120nm thick);

[0067] 2) A first intrinsic amorphous silicon layer (5 nm thick) is deposited on the front side and a second intrinsic amorphous silicon layer (5 nm thick) is deposited on the back side of the above-mentioned N-type single crystal silicon wafer using the PECVD method. Then, a P-type microcrystalline silicon layer (20 nm thick) is deposited on the surface of the first intrinsic amorphous silicon layer and an N-type microcrystalline silicon layer (25 nm thick) is deposited on the surface of the second intrinsic amorphous silicon layer.

[0068] 3) Deposit the TCO film P1 on the surface of the P-type microcrystalline silicon layer of the above silicon wafer (the operation process and parameters are exactly the same as the preparation of the TCO film P1 mentioned above); deposit a back TCO film (100nm thick, material is ICO, i.e. 1% CeO2 + 99% In2O3) on the surface of the N-type microcrystalline silicon layer of the above silicon wafer.

[0069] 4) Place the coated silicon wafer obtained in step 3) into an annealing furnace for annealing at a temperature of 190°C for 30 minutes.

[0070] 5) Using screen printing, a silver electrode is deposited on the mixed layer conductive region of the TCO thin film P1 and on the back TCO thin film (wherein the silver electrode on the front side completely overlaps with the upper surface of the mixed layer conductive region of P1) and cured to obtain a heterojunction solar cell (denoted as B1).

[0071] Example 2

[0072] Preparation of TCO thin films:

[0073] i) Take a clean, smooth glass sheet (75mm × 25mm in size, 1mm in thickness) and place it in the coating machine. Use magnetron sputtering to deposit an ITO (3% by weight SnO2 + 97% by weight In2O3) thin film on the surface of the glass sheet (the gas introduced is a mixture of high-purity argon and high-purity hydrogen, with a partial pressure of 0.4% for high-purity hydrogen, a target power of 2.5KW, and a coating temperature of 180℃) to form the first TCO layer.

[0074] ii) Deposit an ICO (1% by weight CeO2 + 99% by weight In2O3) thin film on the surface of the first TCO layer (the gas introduced is a mixture of high-purity argon, high-purity hydrogen and high-purity oxygen, with the partial pressure of high-purity hydrogen accounting for 1%, the partial pressure of high-purity oxygen gradually increasing from 3% to 10%, the target power is 2.5KW, and the coating temperature is 180℃) to form the second TCO layer;

[0075] iii) A mask is placed above the second TCO layer (the openings of the mask correspond to the deposition positions of the conductive areas), and an ICO (1% by weight CeO2 + 99% by weight In2O3) thin film is deposited on the surface of the second TCO layer through the mask (the gas introduced is a mixture of high-purity argon and high-purity hydrogen, the partial pressure of high-purity hydrogen is 1%, the target power is 2.5KW, and the deposition temperature is 180℃) to form a conductive area; then, a MgF2 thin film is deposited in the space on the surface of the second TCO layer other than the conductive area (using polycrystalline granular raw materials, evaporation by thermal resistance method, slowly adjusting the evaporation current to 90A, pre-melting and then evaporating smoothly) to form an anti-reflection area. The conductive area and the anti-reflection area together form a hybrid layer.

[0076] The resulting composite film was annealed at 190℃ for 30 min to obtain a composite TCO film (denoted as P2).

[0077] In P2, the thickness of the first TCO layer is 6 nm, the thickness of the second TCO layer is 105 nm, and the thickness of the hybrid layer is 150 nm; the thickness ratio of the first TCO layer to the second TCO layer is 1:17.5; the ratio of the contact area between the conductive region and the second TCO layer and the contact area between the antireflection region and the second TCO layer is 0.02:1.

[0078] Fabrication of heterojunction solar cells:

[0079] Following the method of Example 1, except that the TCO thin film P1 is replaced with the above-mentioned TCO thin film P2, and all other conditions are the same as in Example 1, a heterojunction solar cell (denoted as B2) is obtained.

[0080] Example 3

[0081] Preparation of TCO thin films:

[0082] i) Take a clean, smooth glass sheet (75mm × 25mm in size, 1mm in thickness) and place it in the coating machine. Use magnetron sputtering to deposit an ITO (3% by weight SnO2 + 97% by weight In2O3) thin film on the surface of the glass sheet (the gas introduced is a mixture of high-purity argon and high-purity hydrogen, with a partial pressure of 0.4% for high-purity hydrogen, a target power of 2.5KW, and a coating temperature of 180℃) to form the first TCO layer.

[0083] ii) Deposit an ITO (3% SnO2 + 97% In2O3 by weight) thin film on the surface of the first TCO layer (the gas introduced is a mixture of high-purity argon, high-purity hydrogen and high-purity oxygen, with a partial pressure of 1% for high-purity hydrogen and a partial pressure of high-purity oxygen gradually increasing from 3% to 10%, a target power of 2.5KW, and a deposition temperature of 180℃) to form the second TCO layer;

[0084] iii) A mask is placed above the second TCO layer (the openings of the mask correspond to the deposition positions of the conductive areas), and an ITO (3% by weight SnO2 + 97% by weight In2O3) thin film is deposited on the surface of the second TCO layer through the mask (the gas introduced is a mixture of high-purity argon and high-purity hydrogen, the partial pressure of high-purity hydrogen is 1%, the target power is 2.5KW, and the deposition temperature is 180℃) to form a conductive area; then, a MgF2 thin film is deposited in the space on the surface of the second TCO layer other than the conductive area (using polycrystalline granular raw materials, evaporation by thermal resistance method, slowly adjusting the evaporation current to 90A, pre-melting and then evaporating smoothly) to form an anti-reflection area. The conductive area and the anti-reflection area together form a hybrid layer.

[0085] The resulting composite film was annealed at 190℃ for 30 min to obtain a composite TCO film (denoted as P3).

[0086] In P3, the thickness of the first TCO layer is 2nm, the thickness of the second TCO layer is 75nm, and the thickness of the hybrid layer is 100nm; the thickness ratio of the first TCO layer to the second TCO layer is 1:37.5; the ratio of the contact area between the conductive region and the second TCO layer and the contact area between the antireflection region and the second TCO layer is 0.03:1.

[0087] Fabrication of heterojunction solar cells:

[0088] Following the method of Example 1, except that the TCO thin film P1 is replaced with the above-mentioned TCO thin film P3, and all other conditions are the same as in Example 1, a heterojunction solar cell (denoted as B3) is obtained.

[0089] Example 4

[0090] Preparation of TCO thin films:

[0091] i) Take a clean, smooth glass sheet (75mm × 25mm in size, 1mm in thickness) and place it in the coating machine. Use magnetron sputtering to deposit an ITO (3% by weight SnO2 + 97% by weight In2O3) thin film on the surface of the glass sheet (the gas introduced is a mixture of high-purity argon and high-purity hydrogen, with a partial pressure of 0.4% for high-purity hydrogen, a target power of 2.5KW, and a coating temperature of 180℃) to form the first TCO layer.

[0092] ii) Deposit an ITO (3% SnO2 + 97% In2O3 by weight) thin film on the surface of the first TCO layer (the gas introduced is a mixture of high-purity argon, high-purity hydrogen and high-purity oxygen, with a partial pressure of 1% for high-purity hydrogen and a partial pressure of high-purity oxygen gradually increasing from 3% to 10%, a target power of 2.5KW, and a deposition temperature of 180℃) to form the second TCO layer;

[0093] iii) A mask is placed above the second TCO layer (the openings of the mask correspond to the deposition positions of the conductive areas), and an ITO (3% by weight SnO2 + 97% by weight In2O3) thin film is deposited on the surface of the second TCO layer through the mask (the gas introduced is a mixture of high-purity argon and high-purity hydrogen, the partial pressure of high-purity hydrogen is 1%, the target power is 2.5KW, and the deposition temperature is 180℃) to form a conductive area; then, a MgF2 thin film is deposited in the space on the surface of the second TCO layer other than the conductive area (using polycrystalline granular raw materials, evaporation by thermal resistance method, slowly adjusting the evaporation current to 90A, pre-melting and then evaporating smoothly) to form an anti-reflection area. The conductive area and the anti-reflection area together form a hybrid layer.

[0094] The resulting composite film was annealed at 190℃ for 30 min to obtain a composite TCO film (denoted as P4).

[0095] In P4, the thickness of the first TCO layer is 10 nm, the thickness of the second TCO layer is 110 nm, and the thickness of the hybrid layer is 130 nm; the thickness ratio of the first TCO layer to the second TCO layer is 1:11; the ratio of the contact area between the conductive region and the second TCO layer and the contact area between the antireflection region and the second TCO layer is 0.022:1.

[0096] Fabrication of heterojunction solar cells:

[0097] Following the method of Example 1, except that the TCO thin film P1 is replaced with the above-mentioned TCO thin film P4, and all other conditions are the same as in Example 1, a heterojunction solar cell (denoted as B4) is obtained.

[0098] Example 5

[0099] Preparation of TCO thin films:

[0100] Following the method of Example 4, except that the deposition thickness of the mixed layer was changed, while all other conditions were the same as in Example 4, a TCO film (denoted as P5) was obtained;

[0101] In P5, the thickness of the first TCO layer is 10 nm, the thickness of the second TCO layer is 110 nm, and the thickness of the hybrid layer is 110 nm; the thickness ratio of the first TCO layer to the second TCO layer is 1:11; the ratio of the contact area between the conductive region and the second TCO layer and the contact area between the antireflection region and the second TCO layer is 0.022:1.

[0102] Fabrication of heterojunction solar cells:

[0103] Following the method of Example 4, except that the TCO thin film P4 is replaced with the above-mentioned TCO thin film P5, and all other conditions are the same as in Example 4, a heterojunction solar cell (denoted as B5) is obtained.

[0104] Example 6

[0105] Preparation of TCO thin films:

[0106] The method is the same as in Example 4, except that the material of the anti-reflection region is replaced with SiN. x (The tubular PECVD coating process was used, and the gas introduced was a mixture of high-purity SiH4 and high-purity NH3, with an NH3 / SiH4 ratio of 3.34, a target power of 18KW, and a coating temperature of 200℃). Other conditions were the same as in Example 4, and a TCO thin film (denoted as P6) was obtained.

[0107] In P6, the thickness of the first TCO layer is 10 nm, the thickness of the second TCO layer is 110 nm, and the thickness of the hybrid layer is 130 nm; the thickness ratio of the first TCO layer to the second TCO layer is 1:11; the ratio of the contact area between the conductive region and the second TCO layer and the contact area between the antireflection region and the second TCO layer is 0.022:1.

[0108] Fabrication of heterojunction solar cells:

[0109] Following the method of Example 4, except that the TCO thin film P4 is replaced with the above-mentioned TCO thin film P6, and all other conditions are the same as in Example 4, a heterojunction solar cell (denoted as B6) is obtained.

[0110] Example 7

[0111] Preparation of TCO thin films:

[0112] The method of Example 4 is followed, except that the contact area between the conductive region and the second TCO layer and the contact area between the antireflection region and the second TCO layer are changed, while other conditions are the same as in Example 4, to obtain a TCO film (denoted as P7).

[0113] In P7, the thickness of the first TCO layer is 10 nm, the thickness of the second TCO layer is 110 nm, and the thickness of the hybrid layer is 130 nm; the thickness ratio of the first TCO layer to the second TCO layer is 1:11; the ratio of the contact area between the conductive region and the second TCO layer and the contact area between the antireflection region and the second TCO layer is 0.03:1.

[0114] Fabrication of heterojunction solar cells:

[0115] Following the method of Example 4, except that the TCO thin film P4 is replaced with the above-mentioned TCO thin film P7, and all other conditions are the same as in Example 4, a heterojunction solar cell (denoted as B7) is obtained.

[0116] Example 8

[0117] Preparation of TCO thin films:

[0118] The method of Example 4 is followed, except that the total deposition thickness of the first TCO layer, the second TCO layer and the mixed layer is kept the same as in Example 4, and the deposition thickness of the first TCO layer, the second TCO layer and the mixed layer is changed. All other conditions are the same as in Example 4, and a TCO film (denoted as P8) is obtained.

[0119] In P8, the thickness of the first TCO layer is 2nm, the thickness of the second TCO layer is 100nm, and the thickness of the hybrid layer is 148nm; the thickness ratio of the first TCO layer to the second TCO layer is 1:50; the ratio of the contact area between the conductive region and the second TCO layer and the contact area between the antireflection region and the second TCO layer is 0.022:1.

[0120] Fabrication of heterojunction solar cells:

[0121] Following the method of Example 4, except that the TCO thin film P4 is replaced with the above-mentioned TCO thin film P8, and all other conditions are the same as in Example 4, a heterojunction solar cell (denoted as B8) is obtained.

[0122] Comparative Example 1

[0123] Preparation of TCO thin films:

[0124] The method of Example 1 is followed, except that in step iii), an ICO (1% by weight CeO2 + 99% by weight In2O3) thin film is deposited on the surface of the second TCO layer (the gas introduced is a mixture of high-purity argon and high-purity hydrogen, the partial pressure of high-purity hydrogen is 1%, the target power is 2.5KW, and the deposition temperature is 180°C) to form a third TCO film. Other operations and conditions are the same as in Example 1, and a TCO thin film (denoted as DP1) is obtained.

[0125] In DP1, the thickness of the first TCO layer is 4nm, the thickness of the second TCO layer is 80nm, and the thickness of the third TCO layer is 110nm.

[0126] Fabrication of heterojunction solar cells:

[0127] Following the method of Example 1, except that the TCO thin film P1 is replaced with the above-mentioned TCO thin film DP1, and all other conditions are the same as in Example 1, a heterojunction solar cell (denoted as DB1) is obtained.

[0128] Comparative Example 2

[0129] Preparation of TCO thin films:

[0130] i) Take a clean, smooth glass sheet (75mm × 25mm in size, 1mm in thickness) and place it in the coating machine. Use magnetron sputtering to deposit an ICO (1% by weight CeO2 + 99% by weight In2O3) thin film on the surface of the glass sheet (the gas introduced is a mixture of high-purity argon and high-purity hydrogen, with a partial pressure of 0.4% for high-purity hydrogen, a target power of 2.5KW, and a coating temperature of 180℃) to form the first TCO layer.

[0131] ii) Deposit an ICO (1% by weight CeO2 + 99% by weight In2O3) thin film on the surface of the first TCO layer (the gas introduced is a mixture of high-purity argon, high-purity hydrogen and high-purity oxygen, with the partial pressure of high-purity hydrogen accounting for 1%, the partial pressure of high-purity oxygen gradually increasing from 3% to 10%, the target power is 2.5KW, and the coating temperature is 180℃) to form the second TCO layer;

[0132] iii) Deposit an ICO (1% by weight CeO2 + 99% by weight In2O3) thin film on the surface of the second TCO layer (the gas introduced is a mixture of high-purity argon and high-purity hydrogen, the partial pressure of high-purity hydrogen is 1%, the target power is 2.5KW, and the deposition temperature is 180℃) to form a third TCO film.

[0133] iv) A MgF2 thin film is deposited on the surface of the third TCO layer (using polycrystalline granular raw materials, thermal resistance method for evaporation, slowly adjusting the evaporation current to 90A, pre-melting and then evaporating smoothly) to form a MgF2 layer.

[0134] The resulting composite film was annealed at 190℃ for 30 min to obtain a composite TCO film (denoted as DP2).

[0135] In DP2, the thickness of the first TCO layer is 4nm, the thickness of the second TCO layer is 80nm, the thickness of the third TCO layer is 10nm, and the thickness of the MgF2 layer is 100nm.

[0136] Fabrication of heterojunction solar cells:

[0137] Following the method of Example 1, except that the TCO thin film P1 is replaced with the above-mentioned TCO thin film DP2, and all other conditions are the same as in Example 1, a heterojunction solar cell (denoted as DB2) is obtained.

[0138] Test case

[0139] The light transmittance and resistivity of the above TCO films P1-P8 and DP1-DP2 were tested respectively, and the results are shown in Table 1.

[0140] Light transmittance test: The average light transmittance of the TCO film layer was determined by UV-Vis spectrophotometer at 25°C, using a blank glass as a control, according to the method specified in GB / T 30983-2014.

[0141] Conductivity test: The resistivity of the TCO thin film was measured by depositing the thin film onto a glass slide at 25°C according to the method specified in GB / T 4326-2006 and using a Hall effect tester.

[0142] The heterojunction solar cells B1-B8 and DB1-DB2 were subjected to IV tests. A solar simulator was used to simulate sunlight shining on the cells, and a digital source meter was used to test the IV characteristics of the cells. The short-circuit current density and fill factor of the cells were calculated. The results are shown in Table 2.

[0143] Table 1

[0144]

[0145]

[0146] Table 2

[0147]

[0148] As shown in Tables 1 and 2, the composite TCO films P1-P8 provided by this invention adopt a composite structure with a first TCO layer, a second TCO layer, and a hybrid layer. The hybrid layer is divided into a conductive region and an anti-reflection region that are in contact with each other. Compared with traditional TCO films, it can better balance light transmittance and conductivity, and can achieve a light transmittance of not less than 90% in the 400-1100nm wavelength band, while having (2.3-3)×10 -4 The low resistivity of Ω·cm results in higher short-circuit current density and fill factor for heterojunction solar cells, leading to excellent electrical and optical performance. Specifically, the TCO films provided in Comparative Examples 1 and 2 do not possess the structure of the composite TCO film of this invention, and their photoelectric performance is inferior to that of P1-P8.

[0149] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A composite TCO thin film, characterized in that, The composite TCO film comprises a first TCO layer, a second TCO layer, and a hybrid layer stacked sequentially. The hybrid layer includes multiple conductive regions and multiple antireflection regions, and both the conductive regions and the antireflection regions are in contact with the second TCO layer, with the conductive regions and the antireflection regions arranged alternately.

2. The composite TCO film according to claim 1, wherein, The anti-reflection region is made of MgF2 or SiN. x At least one of SiO2, Al2O3, TiO2 and ZnS, preferably MgF2 and SiN x At least one of SiO2.

3. The composite TCO film according to claim 1 or 2, wherein, The materials of the first TCO layer, the second TCO layer, and the conductive region are each independently selected from at least one of IWO, ITO, AZO, ICO, and VTTO.

4. The composite TCO film according to any one of claims 1-3, wherein, The ratio of the contact area between the conductive region and the second TCO layer to the contact area between the antireflection region and the second TCO layer is (0.02-0.03):

1.

5. The composite TCO film according to any one of claims 1-3, wherein, The thickness of the first TCO layer is 2-10 nm, preferably 4-6 nm; And / or, the thickness of the second TCO layer is 70-110 nm, preferably 80-100 nm; And / or, the thickness of the hybrid layer is 80-150 nm, preferably 100-120 nm.

6. The composite TCO film according to any one of claims 1-5, wherein, The thickness ratio of the first TCO layer to the second TCO layer is 1:(7-40).

7. The composite TCO film according to any one of claims 1-6, wherein, The composite TCO film exhibits a light transmittance greater than 90% in the 400-1100nm wavelength band during light transmittance testing.

8. The composite TCO film according to any one of claims 1-6, wherein, The resistivity of the composite TCO thin film is (2.3-3)×10⁻⁶. -4 Ω·cm.

9. A heterojunction solar cell, characterized in that, The heterojunction solar cell includes: an N-type monocrystalline silicon substrate, a first intrinsic amorphous silicon layer, a P-type microcrystalline silicon layer, a first conductive layer and a first metal electrode arranged sequentially from near to far on the front side of the substrate, and a second intrinsic amorphous silicon layer, an N-type microcrystalline silicon layer, a second conductive layer and a second metal electrode arranged sequentially from near to far on the back side of the substrate. Wherein, the first conductive layer is the composite TCO thin film according to any one of claims 1-8, and the first metal electrode contacts and covers the conductive area in the composite TCO thin film.

10. A photovoltaic module comprising the heterojunction solar cell of claim 9.

Citation Information

Patent Citations

  • Transparent conducting assembly for crystalline silicon solar cell and preparation method thereof

    CN105702757A

  • PERC battery with novel front structure

    CN111223945A