Negative electrode material composition, application of carbonate containing alkali metal ions to preparation of negative electrode material of liquid metal battery, liquid metal battery and electric device
By using a carbonate and metallic lithium composition containing alkali metal ions in a liquid metal battery, the problem of contact between the negative electrode current collector and molten lithium is solved, the interface resistance is reduced, the Coulombic efficiency and cycle performance are improved, and the liquid metal is promoted battery development.
Patent Information
- Application Number
- CN202411134232.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-22
AI Technical Summary
In molten lithium metal batteries, it is difficult to maintain good contact between the negative electrode current collector and molten lithium metal. The wettability between molten lithium and the electrolyte is poor, resulting in high battery interface resistance and poor cycle performance, which hinders the further development of molten lithium metal batteries.
Carbonate containing alkali metal ions is used as an additive to combine with metallic lithium to form a negative electrode material composition, which improves the mobility of metallic lithium and its contact performance with the electrolyte and current collector, and reduces the interface resistance.
Through the alloying reaction, the wettability and wettability of the negative electrode material are improved, the interface resistance is significantly reduced, and the Coulombic efficiency and cycle performance of the liquid metal battery are improved.
Smart Images

Figure BDA0005000300260000111 
Figure HDA0005000300420000011 
Figure HDA0005000300420000021
Abstract
Description
Technical Field
[0001] The present application belongs to the field of electrochemical energy storage technology, and in particular relates to a negative electrode material composition and a carbonate containing alkali metal ions for use in preparing a negative electrode material for a liquid metal battery, a liquid metal battery, and an electrical device. Background Art
[0002] In recent years, with the acceleration of my country's energy transformation and upgrading, the construction and planning of modern smart grid systems with energy storage technology and systems as the core have attracted increasing attention. Energy storage technology has been widely used in various aspects of power generation, transmission, distribution, and power consumption. Liquid metal batteries are a new type of energy storage battery that has developed rapidly in recent years. They are composed of automatically layered molten positive electrodes, molten negative electrodes, and electrolytes in a high temperature environment of 300℃ to 700℃. They have the advantages of simple structure, low cost, high current density, and long service life, and have received widespread attention from the large-scale energy storage industry.
[0003] However, in molten lithium metal batteries, there are problems such as the difficulty of maintaining good contact between the negative electrode current collector and the molten metal lithium at high temperatures, poor wettability between the molten lithium and the electrolyte sheet, and the inability of the metal lithium to be spread on the electrolyte surface to obtain good interface contact. The existence of these problems leads to large battery interface resistance and poor cycle performance, hindering the further development of molten lithium metal batteries. Summary of the invention
[0004] The embodiment of the present application provides a negative electrode material composition, which can improve the fluidity of metallic lithium, improve the contact performance between the metallic lithium negative electrode and the electrolyte and the current collector, reduce the interface resistance, and improve the coulombic efficiency of the battery.
[0005] In a first aspect, the present application provides a negative electrode material composition, comprising: metallic lithium, and an additive; the additive comprises a carbonate containing an alkali metal ion, and the mass ratio of the additive to the metallic lithium is 1:(9-49).
[0006] According to an embodiment of the first aspect of the present application, the additive is selected from sodium carbonate, potassium carbonate or a combination thereof.
[0007] According to an embodiment of the first aspect of the present application, the mass ratio of the additive to metallic lithium is 1:(18-25).
[0008] According to an embodiment of the first aspect of the present application, the additive is potassium carbonate, and the mass ratio of potassium carbonate to metallic lithium is 1:(18-20).
[0009] In a second aspect, the present application provides a use of a carbonate containing alkali metal ions for preparing a negative electrode material for a liquid metal battery.
[0010] In a third aspect, the present application provides a liquid metal battery, comprising:
[0011] A battery housing having a hollow receiving cavity;
[0012] A solid electrolyte is disposed in the receiving cavity; the solid electrolyte separates the receiving cavity into a positive electrode region and a negative electrode region;
[0013] The positive electrode region contains positive electrode materials, which include active materials, lithium ion conductive additives, and electron conductive additives;
[0014] The negative electrode region includes the negative electrode material composition and a negative electrode current collector soaked in the negative electrode material composition.
[0015] According to an embodiment of the third aspect of the present application, the volume ratio of the active material, the lithium ion conductive additive, and the electron conductive additive is 5:5-15:7-20.
[0016] According to an embodiment of the third aspect of the present application, the active material includes a lithium-containing halide salt.
[0017] According to an embodiment of the third aspect of the present application, the active substance is selected from lithium fluoride, lithium chloride, lithium bromide, lithium iodide or a combination thereof.
[0018] According to an embodiment of the third aspect of the present application, the lithium ion conductive additive is selected from LiAlCl4, LiZnCl4 or a combination thereof.
[0019] According to an embodiment of the third aspect of the present application, the electronic conductive additive is selected from copper powder, brass powder, zinc, carbon black or a combination thereof.
[0020] According to an embodiment of the third aspect of the present application, the particle size of the electronic additive is 200 mesh to 500 mesh.
[0021] According to an embodiment of the third aspect of the present application, the brass powder is an alloy of zinc and copper, wherein the mass percentage of zinc is 42wt.%, and the mass percentage of copper is 58wt.%.
[0022] According to an embodiment of the third aspect of the present application, the particle size of the brass powder is 200 mesh to 300 mesh.
[0023] According to an embodiment of the third aspect of the present application, the material of the negative electrode current collector is selected from stainless steel, tungsten, molybdenum, nickel, titanium, iron-nickel alloy, and graphite.
[0024] According to an embodiment of the third aspect of the present application, the stainless steel is selected from 304 stainless steel, 316 stainless steel and 446 stainless steel or a composite thereof.
[0025] According to an embodiment of the third aspect of the present application, the solid electrolyte is selected from lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide, lithium aluminum titanium phosphate, lithium lanthanum titanium oxide or a combination thereof.
[0026] In a fourth aspect, the present application provides an electrical device comprising the above-mentioned liquid metal battery.
[0027] The negative electrode material composition of the embodiment of the present application, by adding an additive of carbonate containing alkali metal ions to lithium metal, forms a negative electrode material composition including lithium metal and the additive, which can greatly improve the fluidity of molten metallic lithium, thereby improving the contact performance between the metallic lithium negative electrode and the solid electrolyte and the negative electrode current collector, reducing the interface resistance, and improving the coulombic efficiency of the liquid metal battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solution of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0029] Figure 1 This is a flowability diagram of a molten metal lithium negative electrode material composition formed by combining K2CO3 and metal lithium in a mass ratio of 1:19 provided in Example 1 of the present application.
[0030] Figure 2 This is a physical picture of the wetting condition of the negative electrode current collector and the negative electrode material composition provided in Example 1 of the present application.
[0031] Figure 3 This is an electron microscope image of the interface between the negative electrode material composition provided in Example 1 of the present application and LLZTO as a solid electrolyte, magnified 200 times.
[0032] Figure 4 This is a voltage-time test curve of the molten liquid lithium metal battery of Example 2 of the present application.
[0033] Figure 5 It is a schematic diagram of the structure of the liquid metal battery of an embodiment of the present application.
[0034] Figure 6 It is a schematic structural diagram of a negative electrode current collector according to another embodiment of the present application.
[0035] Figure 7 It is a schematic structural diagram of a negative electrode current collector according to another embodiment of the present application.
[0036] Explanation of the accompanying drawings: 1. battery casing; 10. accommodating cavity; 2. solid electrolyte sheet or solid electrolyte layer; 3. negative electrode region; 31. negative electrode material composition; 32. negative electrode current collector; 32a. main body; 32b. connecting part; 4. positive electrode region; 41. positive electrode material; 5. sealing part. DETAILED DESCRIPTION
[0037] The features and exemplary embodiments of various aspects of the present application will be described in detail below. In order to make the purpose, technical solutions and advantages of the present application clearer, the present application will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only intended to explain the present application, rather than to limit the present application. For those skilled in the art, the present application can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present application by illustrating the examples of the present application.
[0038] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "include..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0039] In the prior art, the solid-solid interface problem caused by the introduction of solid electrolytes will greatly increase the interface impedance. The reason is that compared with organic electrolytes, solid electrolytes have poor fluidity, resulting in poor wettability between the electrode and the electrolyte. At the negative electrode-electrolyte interface, optimizing the electrolyte components can greatly improve the wettability of the interface, and transform the negative electrode / electrolyte interface from lithium-phobic to lithium-philic. In oxide solid electrolytes, experiments have shown that in solid-phase synthesis of oxide electrolytes Li 6.5 LqCy 1.5 Ta 0.5 O 12 Adding 5% Li3PO4 to (LLZTO) can enhance the aggregation of LLZTO particles, increase the solid-solid contact area, and improve the interface wettability. On the basis of optimizing the electrolyte, surface treatment of the interface can also effectively improve the wettability of the interface. For example, Mg is deposited on the electrolyte using atomic deposition layer (ALD). The heat generated by subsequent heat treatment and charge and discharge process will cause Mg to dissolve and diffuse into Li to form a Li-Mg alloy negative electrode. The alloy negative electrode can be in a spreading state on the electrolyte surface, improving the interface wettability, thereby accelerating the interface ion transfer rate and reducing the interface impedance.
[0040] In order to solve the problems existing in the prior art, the embodiments of the present application provide a negative electrode material composition, a liquid metal battery, an electrical device, and a carbonate containing alkali metal ions for use in preparing a negative electrode material. The negative electrode material composition provided in the embodiments of the present application is first introduced below.
[0041] In a first aspect, the negative electrode material composition provided in the embodiments of the present application includes: metallic lithium, and an additive; the additive includes a carbonate containing an alkali metal ion.
[0042] The negative electrode material composition of the embodiment of the present application, by adding an additive including a carbonate containing alkali metal ions to lithium metal, that is, forming a negative electrode material composition including lithium metal and the additive, can greatly improve the fluidity of molten metallic lithium, thereby improving the contact performance between the metallic lithium negative electrode and the solid electrolyte and the negative electrode current collector, reducing the interface resistance, and improving the coulombic efficiency of the liquid metal battery.
[0043] In the negative electrode material composition of the embodiment of the present application, the metal cations in the carbonate containing alkali metal ions can undergo an alloying reaction with the negative electrode metal lithium, thereby improving the wettability of the negative electrode material, thereby maintaining good contact between the negative electrode material and the negative electrode current collector, and ensuring good wettability between the negative electrode material and the solid electrolyte.
[0044] The contact angle tests were conducted on the negative electrode material composition of the present application and the molten elemental metallic lithium. The contact angle test is to place the molten metallic lithium and the molten metallic lithium with additives on the surface of the ceramic electrolyte respectively, and test their contact angles at 300°C. According to the test, the contact angle of molten metallic lithium, that is, molten elemental metallic lithium, is about 85°. The negative electrode material composition of the embodiment of the present application, taking the addition of potassium carbonate as an example, can reduce the contact angle of the molten metallic lithium containing additives to 20°~28°, so that the negative electrode material composition containing alkali metal ion carbonate can maintain good contact with the negative electrode current collector when used as the negative electrode material, reduce the interface resistance between the molten metallic lithium and the negative electrode current collector when used as the negative electrode, and improve the cycle performance of the liquid metal battery.
[0045] In some embodiments of the present application, the additive is selected from sodium carbonate, potassium carbonate or a combination thereof.
[0046] In some embodiments of the present application, the mass ratio of the additive to the metallic lithium is 1:(9-49). Exemplarily, the mass ratio of the additive to the metallic lithium is 1:10, 1:10.5, 1:11, 1:12, 1:13.5, 1:15, 1:16, 1:17, 1:18, 1:20, 1:21, 1:23, 1:25, 1:27, 1:28, 1:30, 1:32, 1:34, 1:35, 1:38, 1:40, 1:42, 1:43, 1:45, 1:46, 1:47, 1:48, 1:48.5.
[0047] In some embodiments, the mass ratio of the additive to metallic lithium is 1:(18-25).
[0048] In some embodiments of the present application, the additive is potassium carbonate. Optionally, the mass ratio of potassium carbonate to metallic lithium is 1:(18-20).
[0049] In the embodiment of the present application, the melting point of potassium carbonate is 891°C. If the amount of potassium carbonate added is too high, the negative electrode material will become viscous, the fluidity will deteriorate, and it will not be able to wet and contact well with the negative electrode current collector and the solid electrolyte. If the amount of potassium carbonate added is too little, the wettability of the negative electrode material cannot be well improved. Therefore, additives in the mass ratio range of 1: (18 to 20) can effectively improve the wettability of the negative electrode material, thereby improving the coulombic efficiency of the liquid metal battery.
[0050] The existing technology first deposits a metal layer on the surface of the solid electrolyte, and then dissolves the metal layer through heat treatment and diffuses it into the metallic lithium to produce an alloy reaction, or uses the heat generated by the charge and discharge reaction to dissolve the metal and diffuse it into the metallic lithium. The former requires a separate heat treatment procedure, and the latter is in an activated state in the early stage of charge and discharge and has not yet formed an alloy. Therefore, the interface impedance of the liquid metal battery in the first few cycles is large and the coulombic efficiency is low.
[0051] Compared with the prior art, the negative electrode material composition of the embodiment of the present application uses a simple preparation process for the negative electrode material composition of metallic lithium and carbonate containing gold alkali ions. At the operating temperature, the wettability of the negative electrode material composition is always relatively good, and there is no problem of large initial interface impedance, thereby making the coulombic efficiency of the liquid metal battery prepared from the negative electrode material composition stable.
[0052] In some embodiments of the present application, the negative electrode material composition can be prepared by the following preparation steps: a carbonate containing alkali metal ions and metallic lithium are heated and kept at 250° C. to 380° C. for 6 to 60 minutes at a mass ratio of 1: (9 to 49) or 1: (18 to 25) or 1: (18 to 20). Optionally, the heating and keeping time is 25 to 60 minutes.
[0053] In a second aspect, the present application provides a use of a carbonate containing alkali metal ions for preparing a negative electrode material for a liquid metal battery.
[0054] In a third aspect, the present application provides a liquid metal battery, such as Figure 5 As shown, it includes: a battery shell 1, having a hollow accommodating cavity 10; a solid electrolyte 2, arranged in the accommodating cavity 10, dividing the accommodating cavity 10 into a negative electrode area 3 and a positive electrode area 4; wherein the positive electrode area 4 contains a positive electrode material 41, and the positive electrode material includes an active substance, a lithium ion conductive additive, and an electron conductive additive; the negative electrode area 3 includes the above-mentioned negative electrode material composition 31 and a negative electrode current collector 32 impregnated in the negative electrode material composition 31.
[0055] In an embodiment of the present application, a liquid metal battery including a negative electrode material composition, because carbonates containing alkali metal ions are added to the negative electrode material composition, can improve the fluidity of molten metal lithium in the negative electrode region, thereby improving the contact performance between the metal lithium negative electrode and the solid electrolyte, reducing the interface resistance, and improving the coulombic efficiency of the liquid metal battery.
[0056] In some embodiments of the present application, the volume ratio of the active material, the lithium ion conductive additive, and the electron conductive additive is 5:5-15:7-20.
[0057] In some embodiments of the present application, the active material includes a lithium-containing halide salt.
[0058] In some embodiments of the present application, the lithium-containing halide salt is selected from lithium fluoride, lithium chloride, lithium bromide, lithium iodide or a combination thereof.
[0059] In some embodiments of the present application, the lithium ion conductive additive is selected from LiAlCl4, LiZnCl4 or a combination thereof. The lithium ion conductive additive can increase the conduction efficiency of lithium ions.
[0060] In some embodiments of the present application, the electronically conductive additive is selected from copper powder, brass powder, zinc, carbon black or a combination thereof. The electronically conductive additive can increase the conduction rate of electrons.
[0061] In some embodiments of the present application, the particle size of the electronic conductive additive is 200 mesh to 500 mesh. Selecting the electronic conductive additive within this particle size range can accelerate the conduction rate of electrons and maintain stability.
[0062] In some embodiments of the present application, the brass powder is an alloy powder of zinc and copper, wherein the mass percentage of zinc is 42wt.%, and the mass percentage of copper is 58wt.%. For example, the brass powder can be purchased from Stellite Metal Materials Technology Yangzhou Co., Ltd. with a particle size of 300 meshes.
[0063] In the embodiment of the present application, the brass powder meeting the above volume ratio can improve the conductivity of electrons.
[0064] In some embodiments of the present application, the particle size of the brass powder is 200-300 meshes.
[0065] In the embodiments of the present application, the brass powder within the above-mentioned particle size range can further enhance the conduction effect of electrons.
[0066] In some embodiments of the present application, the material of the negative electrode current collector is selected from stainless steel, tungsten, molybdenum, nickel, titanium, iron-nickel alloy, graphite or a combination thereof.
[0067] In some embodiments of the present application, the negative electrode current collector 32 may be formed in one piece using one material or two or more materials and immersed in the negative electrode material composition.
[0068] In other embodiments of the present application, Figure 5 As shown, the negative electrode current collector 32 includes a main body 32a and a connecting portion 32b; the main body 32a is used to connect to an external circuit, and the connecting portion 32b is disposed at the end of the main body 32a located in the negative electrode region 3 and is impregnated in the negative electrode material composition 31. For example, the connecting portion 32b may be in the form of a sheet or a plate extending from the end of the main body 32a to the peripheral side. It is understood that, as Figure 6 As shown, the connecting portion 32b can also be made into a sheet or column shape and distributed at intervals along the radial direction of the main body 32a from the end of the main body 32 in the negative electrode area, or arranged at intervals along the radial and length directions of the main body 32a to increase contact with the negative electrode material composition and ensure that the negative electrode current collector 32 can effectively collect the current.
[0069] In one embodiment, if Figure 5 As shown, the main body of the negative electrode current collector passes through the battery case and is connected to an external circuit, and the main body 32 a and the battery case 1 are sealed and connected by the sealing portion 5 .
[0070] In the embodiments of the present application, nickel, copper, and iron can be made into foam copper, foam iron, and foam nickel, respectively, as negative electrode current collectors. Among them, iron and nickel can also be made into foam nickel iron as negative electrode current collectors. Figure 7 As shown, the connecting portion 32b can be set as the current collector of the above-mentioned foam material, so that the gap of the connecting portion of the foam-like negative electrode current collector in the shape of a foam ball can be filled with and attached to the negative electrode material composition, so as to better wet and contact with the negative electrode material composition in the negative electrode area, thereby reducing the interface impedance between the negative electrode current collector and the negative electrode material composition.
[0071] In some embodiments of the present application, the negative electrode current collector can be made of graphite, including but not limited to rods and strips as the main body of the current collector, and the nickel iron foam made of iron-nickel alloy is arranged at the connecting part at one end of the rod-shaped, graphite main body, and the nickel iron foam is soaked in the negative electrode material composition to achieve the connection between the negative electrode material composition and the negative electrode current collector. It is understandable that the nickel iron foam can be replaced by the above-mentioned iron foam, nickel foam, and copper foam.
[0072] In some embodiments of the present application, the stainless steel is selected from 304 stainless steel, 316 stainless steel, 446 stainless steel, or a composite thereof.
[0073] In the embodiments of the present application, the negative electrode current collector can be immersed in the negative electrode material composition and have good contact with the negative electrode material composition to collect and conduct current, thereby providing a stable current output for the liquid metal battery.
[0074] In some embodiments of the present application, the solid electrolyte is selected from lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide, lithium aluminum titanium phosphate, lithium lanthanum titanium oxide or a combination thereof.
[0075] In the embodiments of the present application, the solid electrolyte may be made into a sheet shape, and the solid electrolyte sheet is formed to separate the cavity to form a positive electrode region and a negative electrode region.
[0076] In the embodiments of the present application, there is no limit to the connection methods of the positive electrode region, negative electrode region, solid electrolyte, battery casing and other components of the liquid metal battery, including but not limited to metal welding, glass sealing, and inorganic salt sealing.
[0077] The operating temperature of the liquid metal battery of the embodiment of the present application is 250°C to 380°C, at which temperature the positive electrode material in the positive electrode region and the negative electrode material composition in the negative electrode region are both in a molten state. By adding an appropriate amount of carbonate containing alkali metal ions to the metallic lithium as the negative electrode material, within this temperature range, the carbonate containing alkali metal ions reacts with the metallic lithium and melts into the molten negative electrode material metallic lithium, that is, an alloying reaction occurs in the metallic lithium, so as to improve the wettability of the negative electrode material including the metallic lithium.
[0078] Optionally, the operating temperature of the liquid metal battery of the embodiment of the present application is 300° C. to 350° C. Within this temperature range, the liquid metal battery has high coulombic efficiency and stable coulombic efficiency.
[0079] Example 1
[0080] This embodiment provides a negative electrode material composition, in which potassium carbonate is used as an additive and added to metallic lithium to verify the effect of the negative electrode material composition on improving the wettability of the negative electrode current collector and the solid electrolyte. The negative electrode material composition is prepared by the following steps:
[0081] (1) 0.03 g of K2CO3 and 0.57 g of metallic Li were weighed in a mass ratio of 1:19. K2CO3 and metallic Li were heated at 300°C for 30 min. The fluidity of metallic lithium was as follows: Figure 1 As shown, it can be seen that metallic lithium is well spread on the solid electrolyte sheet LLZTO.
[0082] (2) Adding nickel iron foam to the negative electrode material composition as the negative electrode current collector, and observing the wetting between the negative electrode current collector and the metal lithium. Figure 2 As shown, Figure 2 The part between the black iron metal rod and the silvery white sphere is the negative electrode current collector. The silvery white sphere is a negative electrode material composition containing metallic lithium and additives, which is evenly filled and attached to the gaps in the foamed nickel iron current collector. The lithium in the negative electrode material composition has a good contact effect with the negative electrode current collector. If the wettability of the negative electrode material is poor, the negative electrode material will not be evenly attached to the negative electrode current collector.
[0083] (3) The interface contact between the negative electrode material composition and the LLZTO solid electrolyte was tested by SEM to observe the interface contact. Figure 3 The upper middle layer is a lithium-containing negative electrode material composition, and the lower layer is a LLZTO solid electrolyte sheet. Figure 3 As shown, the contact interface between the lithium-containing negative electrode material composition and the LLZTO solid electrolyte is relatively flat and uniform, indicating that the negative electrode material composition after adding the additive is in good contact with LLZTO.
[0084] Example 2
[0085] This embodiment provides an application of a negative electrode material composition comprising a carbonate of an alkali metal ion and metallic lithium in a molten liquid metal lithium battery. The molten liquid metal lithium battery, with a specification of 2Ah, is prepared according to the following steps:
[0086] The negative electrode material composition of Example 1 (wherein the mass ratio of K2CO3:Li=1:19) was used as the negative electrode material, LLZTO was used as the solid electrolyte, and a mixture of LiCl, LiAlCl4 and brass powder in a mass ratio of 11.38:31.4:165.8 was used as the positive electrode material to assemble a molten liquid lithium metal battery. The densities of LiCl, LiAlCl4 and brass powder were 2.07 g / cm 3 , 2g / cm 3 、8.29g / cm 3Calculation. Brass powder is an alloy powder of zinc and copper, the mass percentage of zinc is 42wt.%, the mass percentage of copper is 58wt.%, and the particle size of brass powder is 300 mesh. It should be noted that the volumes of LiCl, LiAlCl4 and brass powder in the above mass ratios in the molten liquid metal lithium battery meet the volume ratio restrictions of active material, lithium ion conductive additive and electron conductive additive of 5:5 to 15:7 to 20. The volumes of LiCl, LiAlCl4 and brass powder that meet the above mass ratios in the molten liquid metal lithium battery can be estimated based on their densities in the solid state at room temperature, or their volumes can be measured at a set temperature.
[0087] As shown in Table 1, the coulombic efficiency of the liquid metal battery of Example 2 is 99.98%, which is close to 100%, indicating that the liquid metal battery is fully discharged without the formation of inert lithium. Figure 4 The voltage-time curve of the present embodiment 2 is shown in FIG. Figure 4 As shown, when the charging cut-off voltage reaches 2.6V, the battery capacity reaches the maximum, that is, about 1500mAh; when the discharge voltage reaches 1.6V, the discharge capacity of the battery also reaches nearly 1500mAh.
[0088] Example 3
[0089] Example 3 provides a molten liquid metal lithium battery, which differs from Example 2 in that the mass ratio of the additive Na2CO3 to the metal lithium in the negative electrode material composition is 1:19.
[0090] Example 4
[0091] Example 4 provides a molten liquid metal lithium battery, which differs from Example 2 in that the mass ratio of the additive K2CO3 to the metal lithium in the negative electrode material composition is 1:10.
[0092] Example 5
[0093] Example 5 provides a molten liquid metal lithium battery, which differs from Example 2 in that the mass ratio of the additive K2CO3 to the metal lithium in the negative electrode material composition is 1:30.
[0094] Example 6
[0095] Example 6 provides a molten liquid metal lithium battery, which differs from Example 2 in that the additive in the negative electrode material composition includes K2CO3 and Na2CO3 in a mass ratio of 1:1, and the mass ratio of the additive to metallic lithium is 1:20.
[0096] Comparative Example 1
[0097] Comparative Example 1 provides a molten liquid metal lithium battery, which differs from Example 2 in that the content of the additive K2CO3 in the negative electrode material composition is 0.
[0098] Comparative Example 2
[0099] Comparative Example 2 provides a molten liquid metal lithium battery, which differs from Example 2 in that a layer of metal Ag with a thickness of 200 nm is deposited on the surface of the LLZTO solid electrolyte to obtain a molten liquid metal lithium battery.
[0100] The molten liquid metal lithium batteries of Examples 2-6 and Comparative Examples 1-2 were charged and discharged using an electrochemical testing system to measure the cycle performance and coulombic efficiency of the corresponding molten liquid lithium metal batteries. The test conditions for the charge and discharge tests are as follows: the charge cut-off voltage is 2.6V, and the discharge cut-off voltage is 1.6V; the liquid metal lithium batteries of Examples 2-6 and Comparative Examples 1-2 are activated for one cycle under the condition of a test current of 0.05C, and then charged and discharged at a current of 0.5C, and the test temperature is 350°C. The comparison conditions and coulombic efficiency test data of Examples 2-6 and Comparative Examples 1-2 are recorded in Table 1 below:
[0101] Table 1
[0102]
[0103] By comparing the test data of Coulomb efficiency in Table 1, it can be concluded that:
[0104] As shown in the cycle data of Comparative Example 1, the coulombic efficiency of the liquid metal battery without additives decreases with the increase of the number of cycles since the start of the cycle, and the coulombic efficiency after 2 weeks of circulation is reduced to 67.17%, a decrease of 16.05%; the coulombic efficiency after 3 weeks of circulation is reduced to 43.24%, a decrease of 45.96%. The decrease in a single cycle is about 20%.
[0105] As shown in the cycle data of Comparative Example 2, the liquid metal battery with a metal Ag layer formed on the surface of the solid electrolyte has a poor coulombic efficiency in the initial cycle and needs to be cycled 2-3 times before it can maintain a stable coulombic efficiency.
[0106] The liquid metal batteries of embodiments 2-6 of the present application respectively add corresponding additives, and have a high coulombic efficiency at the beginning of the cycle, and can form a stable output performance without the need for initial cycles. Moreover, the coulombic efficiency of the liquid metal battery of the embodiment of the present application can still maintain a relatively stable coulombic efficiency after 2 to 3 weeks of circulation, and the maximum drop in coulombic efficiency is only 3.56%, indicating that the liquid metal battery with additives added in the embodiment of the present application has good cycle stability.
[0107] From the above comparison, it can be seen that adding an additive containing carbonate of alkali metal ions to lithium metal, that is, forming a negative electrode material composition containing lithium metal and the additive, can greatly improve the fluidity of molten lithium metal, thereby improving the contact performance between the metal lithium negative electrode and the solid electrolyte and the negative electrode current collector, reducing the interface resistance and improving the coulombic efficiency of the liquid metal battery.
[0108] The above is only a specific implementation method of the present application. Those skilled in the art can clearly understand that for the convenience and simplicity of description, the specific working process described above can refer to the corresponding process in the aforementioned method embodiment, and will not be repeated here. It should be understood that the protection scope of the present application is not limited to this. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in the present application, and these modifications or replacements should be included in the protection scope of the present application.
Claims
1. A negative electrode material composition, characterized in that: include: Metallic lithium, and an additive; the additive comprises a carbonate containing an alkali metal ion, and the mass ratio of the additive to the metallic lithium is 1:(9-49).
2. The negative electrode material composition according to claim 1, characterized in that: The mass ratio of the additive to the metallic lithium is 1:(18-25).
3. The negative electrode material composition according to claim 1 or 2, characterized in that: The additive is selected from sodium carbonate, potassium carbonate or a combination thereof.
4. The negative electrode material composition according to claim 1 or 2, characterized in that: The additive is potassium carbonate, and the mass ratio of the potassium carbonate to metallic lithium is 1:(18-20).
5. Use of a carbonate containing alkali metal ions for preparing negative electrode materials for liquid metal batteries.
6. A liquid metal battery, characterized in that: include: A battery housing having a hollow receiving cavity; A solid electrolyte is disposed in the containing cavity, and divides the containing cavity into a positive electrode region and a negative electrode region; wherein the positive electrode region contains a positive electrode material, and the positive electrode material includes an active substance, a lithium ion conductive additive, and an electron conductive additive; The negative electrode region comprises the negative electrode material composition as claimed in any one of claims 1 to 4 and a negative electrode current collector impregnated in the negative electrode material composition.
7. The liquid metal battery according to claim 6, characterized in that: The volume ratio of the active material, the lithium ion conductive additive, and the electron conductive additive is 5:5-15:7-20; The active material comprises a lithium-containing halide salt; and / or The lithium ion conductive additive is selected from LiAlCl4, LiZnCl4 or a combination thereof; and / or The electronically conductive additive is selected from copper powder, brass powder, zinc, carbon black or a combination thereof; and / or The negative electrode current collector is made of a material selected from stainless steel, tungsten, molybdenum, nickel, titanium, iron-nickel alloy, and graphite; and / or The solid electrolyte is selected from lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide, lithium aluminum titanium phosphate, lithium lanthanum titanium oxide or a combination thereof.
8. The liquid metal battery according to claim 8, characterized in that: The active substance is selected from lithium fluoride, lithium chloride, lithium bromide, lithium iodide or a combination thereof; and / or The particle size of the electronic conductive additive is 200-500 meshes.
9. The liquid metal battery according to claim 8, characterized in that: The brass powder is an alloy of zinc and copper, wherein the mass percentage of zinc is 42wt.%, and the mass percentage of copper is 58wt.%; and / or The particle size of the brass powder is 200-300 meshes.
10. An electrical device, characterized in that: The electrical device comprises the liquid metal battery as described in any one of claims 6 to 9.