Electrode and solid electrolyte integrated cell, preparation method thereof and battery

By adopting the structure of composite electrode and solid electrolyte in the solid-state sodium ion battery, the problem of large interface impedance between the solid electrolyte and the electrode is solved, the close contact between the electrode and the solid electrolyte is achieved, and the sodium ion transmission rate and the stability of the battery are improved. Security.

CN118825433APending Publication Date: 2024-10-22KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311146244.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-09-06
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In solid-state sodium-ion batteries, the interface resistance between the solid electrolyte and the electrode is large, resulting in uneven sodium ion transmission and affecting the stability and safety of the battery.

Method used

It adopts the structure of composite positive electrode layer, composite negative electrode layer and composite solid electrolyte, containing a specific proportion of positive electrode active material, negative electrode active material, conductive agent, sodium ion conductor and inorganic filler. Through the combination of polymer matrix and sodium salt, a tight Electrode/solid electrolyte interface to reduce interface impedance.

Benefits of technology

It achieves continuous and close contact between the electrode and the solid electrolyte, reduces the interface impedance, increases the sodium ion transmission rate, enhances the stability and safety performance of the battery, and improves the electrochemical performance and service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825433A_ABST
    Figure CN118825433A_ABST
Patent Text Reader

Abstract

The invention discloses an electrode and solid electrolyte integrated cell, a preparation method thereof and a battery. The electrode and solid electrolyte integrated cell comprises a composite positive electrode layer, a composite negative electrode layer and a composite solid electrolyte layer arranged between the composite negative electrode layer and the composite positive electrode layer; wherein the composite positive electrode layer comprises a positive electrode active material, a first binder, a first conductive agent and a first sodium ion conductor; the composite negative electrode layer comprises a negative electrode active material, a second binder, a second conductive agent and a second sodium ion conductor; the composite solid electrolyte comprises a polymer matrix, an inorganic filler and a sodium salt. The electrode and solid electrolyte integrated cell structure disclosed by the invention has a contact interface in close connection, and can reduce the interface impedance between the electrode and the solid electrolyte and improve the sodium ion flux at the interface, thereby improving the interface stability, the cycle life and the electrochemical performance of the solid sodium ion battery comprising the cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of sodium ion batteries, and more specifically, to an electrode and solid electrolyte integrated battery cell and a preparation method thereof and a battery. Background Art

[0002] Sodium-ion batteries have the advantages of high energy efficiency and abundant resource reserves, making them extremely promising for use in electric vehicles, fixed energy supply systems and mobile power sources. They are considered to be the best candidate to replace lithium-ion batteries in the future large-scale energy storage field. Traditional sodium-ion batteries based on organic liquid electrolytes have problems such as electrolyte leakage, flammability and poor thermal stability. The use of solid electrolytes to replace traditional organic electrolytes can solve safety issues such as combustion and explosion caused by electrolyte volatilization and leakage. At the same time, solid electrolytes have good thermal stability and high mechanical strength, making solid-state sodium-ion batteries promising for matching high-energy positive electrodes with metallic sodium negative electrodes. However, the interface wettability of solid electrolytes is poor, and the small solid-solid contact area with the electrode results in a large interface impedance. In addition, the interface impedance between electrode particles restricts the development and application of solid-state batteries. Summary of the invention

[0003] In view of the deficiencies in the prior art, one of the purposes of the present invention is to solve the problems in the prior art. Therefore, the present invention provides a battery cell that can improve the interface contact between the electrode and the solid electrolyte and the positive and negative electrodes and the solid electrolyte.

[0004] On the one hand, the present invention provides an electrode and solid electrolyte integrated battery cell, comprising a composite positive electrode layer, a composite negative electrode layer, and a composite solid electrolyte arranged between the composite negative electrode layer and the composite positive electrode layer, wherein the composite positive electrode layer comprises a positive electrode active material, a first binder, a first conductive agent and a first sodium ion conductor material; the composite negative electrode layer comprises a negative electrode active material, a second binder, a second conductive agent and a second sodium ion conductor material; the composite solid electrolyte comprises a polymer matrix, an inorganic filler and a sodium salt.

[0005] Furthermore, the mass percentage of each component in the composite negative electrode layer is: 30% to 80% of the negative electrode active material, 1% to 20% of the second binder, 1% to 20% of the second conductive agent, and 1% to 20% of the second sodium ion conductor.

[0006] Furthermore, the mass percentage of each component in the composite positive electrode layer is: 30% to 80% of the positive electrode active material, 1% to 20% of the first binder, 1% to 20% of the first conductive agent, and 1% to 20% of the first sodium ion conductor.

[0007] Furthermore, the mass percentage of each component in the composite solid electrolyte is: 25% to 90% of the polymer matrix, 1% to 70% of the inorganic filler; the molar ratio of the sodium salt to the polymer monomer is (0.1 to 1):20.

[0008] Furthermore, the positive electrode active material is selected from Na 1-x FeO2、Na 1-x [Fe 1-x Mn x ]O2(x≤0.5),Na 1- x CoO2、Na 0.7 [(Fe 0.5 Mn 0.5 ) 1-x Co x ]O2、Na x MnO2、Na 2 / 3 [Co 1-x Mn x ]O2、Na 2 / 3x Ca x CoO2、Na 1-x NiO2, Na[Ni 0.75x Fe x Mn 0.25 ]O2、Na 1-x TiO2、Na 1-x CrO2、Na 1-x VO2、Na 2 / 3 [Ni 1 / 3x Mg x Mn 0.7 ]O2、Na 2 / 3 [Ni 1 / 3x Zn x Mn 2 / 3 ]O2、Na 2 / 3 [Ni 1 / 3 Mn 2 / 3x Ti x ]O2、Na 1-x FePO4, Na3V2(PO4)3, Na x [Fe 0.5 Mn 0.5 ]PO4、Na 2- x FePO4F 1-y 、NaVPO4F 1-x 、Na3Fe2(PO4)2F 3-x, at least one of Na4M3(PO4)2P2O7 (M: Mn, Fe, Co, Ni), NaMSO4F (M: Fe, Co, Mn), Na3MPO4CO3 (M: Mg, Mn, Fe, Co, Ni, Cu), Prussian blue, and Prussian white;

[0009] The negative electrode active material is selected from hard carbon, graphite, TiO2, Na 3–x Ti3O7、Na 2+x Ti6O 13 , NiCo2O4, SnO, SnO2, CuO, MS (M: Mn, Fe, Co, Ti, Cu, Sn, Mo, W), MS2 (M: Mn, Fe, Co, Ti, Cu, Sn, Mo, W), MP (M: Ni, Fe, Co, Cu, Sn);

[0010] The first conductive agent and the second conductive agent are both selected from at least one of graphite, graphene, carbon nanotubes, and acetylene black;

[0011] The first sodium ion conductor and the second sodium ion conductor are both selected from Na 1+x Zr2Si x P 3-x O 12 (0≤x≤3), NaMM′P3O 12 (M and M' are Si 2+ ,Mg 2+ , Cu 2+ ,Co 2+ , Zn 2+ , Mn 2+ , Fe 2+ , Al 3+ ,Cr 3+ , Sc 3+ , Y 3+ , La 3 + , Ti 4+ , Zr 4+ ,Ge 4+ , Sn 4+ , Nb 4+ , V 5+ , Nb 5+ , 5+ the same element or different elements), β″-Al2O3, β-Al2O3, Na3PS4, Na3SbS4, Na 11 Sn2PS 12 、Na4Sn 0.67 Si 0.33 At least one of S4 and SN-NaClO4 complexes.

[0012] The first binder and the second binder are both selected from at least one of PEO, PAN, PMMA, PVA, PVP, PVDF, PVDF-HFP, PPC, and PEC;

[0013] Furthermore, the inorganic filler is selected from Si, AlCl3, BaTiO3, CuO, SiO2, ZrO2, TiO2, Na 1+ x Zr2Si x P 3-x O 12 (0≤x≤3), NaMM′P3O 12 (M and M' are Si 2+ ,Mg 2+ , Cu 2+ ,Co 2+ , Zn 2+ , Mn 2+ , Fe 2+ , Al 3+ ,Cr 3+ , Sc 3+ , Y 3+ , La 3+ , Ti 4+ , Zr 4+ ,Ge 4+ , Sn 4+ , Nb 4+ , V 5+ , Nb 5+ , 5+ the same element or different elements), β″-Al2O3, β-Al2O3, Na3PS4, Na3SbS4, Na 11 Sn2PS 12 、Na4Sn 0.67 Si 0.33 At least one of S4;

[0014] The sodium salt is selected from at least one of NaClO4, NaPF6, NaAsF6, NaBF4, NaTFSI, NaTf, NaFSI, and sodium bis(oxalate)borate;

[0015] The polymer matrix is ​​selected from at least one of PEO, PAN, PMMA, PVA, PVP, SN, PVDF, PVDF-HFP, PPC, PEC, and PEG;

[0016] Another aspect of the present invention also provides a method for preparing an electrode and solid electrolyte integrated battery cell, comprising the following steps: mixing a polymer matrix, an inorganic filler, a sodium salt and a first organic solvent to obtain a composite solid electrolyte slurry; coating the composite solid electrolyte slurry on a polytetrafluoroethylene mold, and drying it with air blast to obtain a composite solid electrolyte film; mixing a negative electrode active material, a second binder, a second conductive agent, a second organic solvent and a second sodium ion conductor to obtain a composite negative electrode slurry, coating the composite negative electrode slurry on the composite solid electrolyte film, and drying it with air blast to obtain a laminated structure of a composite negative electrode layer and a composite solid electrolyte; mixing a positive electrode active material, a first binder, a first conductive agent, a third organic solvent and a first sodium ion conductor to obtain a composite positive electrode slurry, coating the composite positive electrode slurry on a side of the composite solid electrolyte film away from the composite negative electrode layer, and drying it with air blast and vacuum drying to obtain an electrode and solid electrolyte integrated battery cell.

[0017] Furthermore, the first organic solvent, the second organic solvent or the third organic solvent comprises one or a combination of acetone, N,N-dimethylformyl (DMF) and nitrogen methyl pyrrolidone (NMP).

[0018] Furthermore, the mass percentage of each component in the composite negative electrode layer is: 30% to 80% of the negative electrode active material, 1% to 20% of the second binder, 1% to 20% of the second conductive agent, and 1% to 20% of the second sodium ion conductor; the mass percentage of each component in the composite positive electrode layer is: 30% to 80% of the positive electrode active material, 1% to 20% of the first binder, 1% to 20% of the first conductive agent, and 1% to 20% of the first sodium ion conductor; the mass percentage of each component in the composite solid electrolyte is: 25% to 90% of the polymer matrix, and 1% to 70% of the inorganic filler; the molar ratio of the sodium salt to the polymer monomer is (0.1 to 1):20.

[0019] Another aspect of the present invention further provides a solid-state sodium ion battery, comprising an electrode and solid electrolyte integrated battery cell prepared by the aforementioned method for preparing an electrode and solid electrolyte integrated battery cell.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The electrode and solid electrolyte integrated battery cell of the present invention has a continuous and tight electrode / solid electrolyte interface, which can reduce the interface impedance between the electrode and the solid electrolyte and improve the uniform sodium ion flux at the interface, thereby achieving high interface stability of the sodium ion battery, thereby avoiding safety problems such as combustion and explosion caused by electrolyte leakage or volatilization, and improving the stability and safety performance of the battery.

[0022] (2) The solid electrolyte and electrode interface impedance in the electrode and solid electrolyte integrated battery cell prepared by the present invention is small, the sodium ion transmission rate is high, and the assembled battery has good electrochemical performance.

[0023] (3) The sodium ion battery assembled with the electrode and solid electrolyte integrated battery cell of the present invention can improve the stability and service life of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The above and other objects and / or features of the present invention will become more apparent through the following description in conjunction with the accompanying drawings, in which:

[0025] Figure 1 It is a schematic diagram of a method for preparing an electrode and solid electrolyte integrated battery cell in an embodiment of the present invention.

[0026] Figure 2 A “cross-section” SEM image of the integrated solid battery core prepared in Example 1 of the present invention is shown.

[0027] Figure 3 The electrochemical impedance diagrams of the batteries of Example 1, Example 2, Example 3 and Comparative Example 1 of the present invention are shown.

[0028] Figure 4 The electrochemical impedance diagrams of the batteries of Example 4, Example 5, Comparative Example 2 and Comparative Example 3 of the present invention are shown.

[0029] Figure 5 The charge-discharge cycle curves of the batteries of Example 1, Example 2 and Comparative Example 1 of the present invention are shown.

[0030] Figure 6 The charge-discharge cycle curves of the batteries of Example 3, Example 4 and Comparative Example 2 of the present invention are shown. DETAILED DESCRIPTION

[0031] Hereinafter, the electrode and solid electrolyte integrated battery cell and the preparation method thereof and the battery of the present invention will be described in detail in conjunction with exemplary embodiments.

[0032] For solid-state sodium-ion batteries, the solid battery cell that integrates electrode materials and solid electrolytes can better solve the problems of large interface impedance between solid electrolytes and electrodes and uneven distribution of sodium ion transmission channels. In addition, solid-state sodium-ion batteries assembled with solid battery cells that integrate electrode materials and solid electrolytes have the advantages of high energy density and small size, providing strong conditions for realizing high energy density batteries and miniaturized batteries.

[0033] An embodiment of the present invention provides a method for preparing an electrode and solid electrolyte integrated battery cell. One basis for the technical concept of the method is that the positive electrode and the negative electrode are in continuous and close contact with the solid electrolyte to reduce the interface impedance and uniform deposition of sodium ions, thereby improving the electrochemical performance of the battery.

[0034] One aspect of the present invention provides an electrode and solid electrolyte integrated battery cell. In this embodiment, the electrode and solid electrolyte integrated battery cell includes a composite negative electrode layer, a composite solid electrolyte and a composite positive electrode layer, and the composite negative electrode layer and the composite positive electrode layer are respectively connected to the two sides of the composite solid electrolyte, so the battery cell structure is a composite negative electrode, a composite positive electrode and a composite solid electrolyte integrated battery cell.

[0035] Wherein, the composite negative electrode layer comprises a negative electrode active material, a second binder, a second conductive agent and a second sodium ion conductor material;

[0036] The composite positive electrode layer comprises a positive electrode active material, a first binder, a first conductive agent and a first sodium ion conductor material;

[0037] The composite solid electrolyte comprises a polymer matrix, an inorganic filler and a sodium salt.

[0038] Wherein, the mass percentage of each component in the composite negative electrode layer is: 30% to 80% of the negative electrode active material, 1% to 20% of the second binder, 1% to 20% of the second conductive agent, and 1% to 20% of the second sodium ion conductor. It can be understood that the mass percentage of the negative electrode active material in the composite negative electrode layer can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, or other percentages within the above range; the mass percentage of the second binder in the composite negative electrode layer can be 1%, 2%, 5%, 7%, 9%, 10%, 12%, 15%, 17%, 18%, 19%, 20%, or other percentages within the above range. content; the mass percentage of the second conductive agent in the composite negative electrode layer can be 1%, 3%, 5%, 7%, 8%, 10%, 12%, 14%, 16%, 18%, 19%, 20%, or other percentages within the above range; the mass percentage of the second sodium ion conductor in the composite negative electrode layer can be 1%, 3%, 5%, 7%, 8%, 10%, 12%, 14%, 16%, 18%, 19%, 20%, or other percentages within the above range.

[0039] Specifically, the negative electrode active material of the composite negative electrode layer is hard carbon, graphite, TiO2, Na 3–x Ti3O7、Na 2+ xTi6O 13 , NiCo2O4, SnO, SnO2, CuO, MS (M: Mn, Fe, Co, Ti, Cu, Sn, Mo, W), MS2 (M: Mn, Fe, Co, Ti, Cu, Sn, Mo, W), MP (M: Ni, Fe, Co, Cu, Sn) or a combination of several thereof.

[0040] The mass percentage of each component in the composite positive electrode layer is: 30% to 80% of positive electrode active material, 1% to 20% of the first binder, 1% to 20% of the first conductive agent, and 1% to 20% of the first sodium ion conductor. It can be understood that the mass percentage of the positive electrode active material in the composite positive electrode layer can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, or other percentages within the above range; the mass percentage of the first binder in the composite positive electrode layer can be 1%, 2%, 4%, 6%, 8%, 10%, 13%, 15%, 17%, 18%, 19%, 20%, or other percentages within the above range. content; the mass percentage of the first conductive agent in the composite positive electrode layer can be 1%, 2%, 4%, 6%, 8%, 10%, 11%, 13%, 15%, 17%, 19%, 20%, or other percentages within the above range; the mass percentage of the first sodium ion conductor in the composite positive electrode layer can be 1%, 3%, 5%, 7%, 8%, 10%, 12%, 14%, 16%, 18%, 19%, 20%, or other percentages within the above range.

[0041] Specifically, the positive electrode active material of the composite positive electrode layer is Na 1-x FeO2、Na 1-x [Fe 1-x Mn x ]O2(x≤0.5),Na 1-x CoO2、Na 0.7 [(Fe 0.5 Mn 0.5 ) 1-x Co x ]O2、Na x MnO2、Na 2 / 3 [Co 1-x Mn x ]O2、Na 2 / 3x Ca x CoO2、Na 1-x NiO2, Na[Ni 0.75x Fe x Mn 0.25 ]O2、Na 1-xTiO2、Na 1-x CrO2、Na 1-x VO2、Na 2 / 3 [Ni 1 / 3x Mg x Mn 0.7 ]O2、Na 2 / 3 [Ni 1 / 3x Zn x Mn 2 / 3 ]O2、Na 2 / 3 [Ni 1 / 3 Mn 2 / 3x Ti x ]O2、Na 1-x FePO4, Na3V2(PO4)3, Na x [Fe 0.5 Mn 0.5 ]PO4、Na 2- x FePO4F 1-y 、NaVPO4F 1-x 、Na3Fe2(PO4)2F 3-x , Na4M3(PO4)2P2O7(M: Mn, Fe, Co, Ni), NaMSO4F(M: Fe, Co, Mn), Na3MPO4CO3(M: Mg, Mn, Fe, Co, Ni, Cu), Prussian blue, and Prussian white, one or a combination of them.

[0042] The mass percentage of each component in the composite solid electrolyte is: 25% to 90% of the polymer matrix, 1% to 70% of the inorganic filler; the molar ratio of the sodium salt to the polymer monomer is (0.1 to 1): 20. It can be understood that the mass percentage of the polymer matrix in the composite solid electrolyte can be 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, or other percentages within the above range; the mass percentage of the inorganic filler in the composite solid electrolyte can be 1%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 65%, 70%, or other percentages within the above range. The molar ratio of the sodium salt to the polymer monomer may be 0.1:20, 0.3:20, 0.4:20, 0.5:20, 0.6:20, 0.7:20, 0.8:20, 0.9:20, or 1:20, or may be other molar ratios within the above range.

[0043] In this embodiment, the first binder and the second binder are both selected from at least one of polyethylene oxide (PEO), polyacrylonitrile (PAN), poly(methyl methacrylate) (PMMA), poly(vinyl alcohol) (PVA), polyvinyl pyrrolidone (PVP), polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), polypropylene carbonate (PPC), and polyethylene carbonate (PEC).

[0044] The first conductive agent and the second conductive agent are both selected from one or a combination of graphite, graphene, carbon nanotubes, and acetylene black.

[0045] The first sodium ion conductor and the second sodium ion conductor are both selected from Na 1+x Zr2Si x P 3-x O 12 (0≤x≤3), NaMM′P3O 12 (M and M' are Si 2+ ,Mg 2+ , Cu 2+ ,Co 2+ , Zn 2+ , Mn 2+ , Fe 2+ , Al 3+ ,Cr 3+ , Sc 3+ , Y 3+ , La 3+ , Ti 4+ , Zr 4+ ,Ge 4+ , Sn 4+ , Nb 4+ , V 5+ , Nb 5+ , 5+ the same element or different elements), β″-Al2O3, β-Al2O3, Na3PS4, Na3SbS4, Na 11 Sn2PS 12 、Na4Sn 0.67 Si 0.33 S4, SN-NaClO4 complex or a combination of several thereof.

[0046] The inorganic filler is Si, AlCl3, BaTiO3, CuO, SiO2, ZrO2, TiO2, Na 1+x Zr2Si x P 3-x O 12 (0≤x≤3), NaMM′P3O 12 (M and M' are Si 2+,Mg 2+ , Cu 2+ ,Co 2+ , Zn 2+ , Mn 2+ , Fe 2+ , Al 3+ ,Cr 3+ , Sc 3+ , Y 3+ , La 3+ , Ti 4+ , Zr 4+ ,Ge 4+ , Sn 4+ , Nb 4+ , V 5+ , Nb 5+ , 5+ the same element or different elements), β″-Al2O3, β-Al2O3, Na3PS4, Na3SbS4, Na 11 Sn2PS 12 、Na4Sn 0.67 Si 0.33 One or a combination of S4.

[0047] In this embodiment, the polymer matrix is ​​one or a combination of PEO, PAN, PMMA, PVA, PVP, SN, PVDF, PVDF-HFP, PPC, PEC, and PEG.

[0048] The sodium salt is one or a combination of NaClO4, NaPF6, NaAsF6, NaBF4, NaTFSI, NaTf, NaFSI, and sodium borate oxalate.

[0049] In some embodiments, the electrode and solid electrolyte integrated battery cell provided by the present invention is a solid-state sodium ion battery cell material.

[0050] See also Figure 1 , Figure 1 Schematic diagram of a method for preparing an electrode and solid electrolyte integrated battery cell in an embodiment of the present invention. Another aspect of the present invention further provides a method for preparing an electrode and solid electrolyte integrated battery cell, comprising the following steps:

[0051] S1, mixing a polymer matrix, an inorganic filler, a sodium salt and a first organic solvent to obtain a composite solid electrolyte slurry;

[0052] S2, coating the composite solid electrolyte slurry on a polytetrafluoroethylene mold, and drying with air blast to obtain a composite solid electrolyte film;

[0053] S3, mixing the negative electrode active material, the second binder, the second conductive agent, the second organic solvent and the second sodium ion conductor to obtain a composite negative electrode slurry;

[0054] S4, coating the composite negative electrode slurry on the composite solid electrolyte film, and drying with air blast to obtain a laminated structure of a composite negative electrode layer and a composite solid electrolyte;

[0055] S5, mixing the positive electrode active material, the first binder, the first conductive agent, the third organic solvent and the first sodium ion conductor to obtain a composite positive electrode slurry;

[0056] S6, coating the composite positive electrode slurry on the side of the composite solid electrolyte film away from the composite negative electrode layer, drying with air blast, and then vacuum drying to obtain an electrode and solid electrolyte integrated battery cell.

[0057] In this embodiment, the content of each component raw material added in the above preparation method is adapted to the content of the components contained in the above-mentioned electrode and solid electrolyte integrated battery cell, that is, the mass percentage of each component in the composite negative electrode layer is: 30% to 80% of the negative electrode active material, 1% to 20% of the second binder, 1% to 20% of the second conductive agent, 1% to 20% of the second sodium ion conductor; the mass percentage of each component in the composite positive electrode layer is: 30% to 80% of the positive electrode active material, 1% to 20% of the first binder, 1% to 20% of the first conductive agent, 1% to 20% of the first sodium ion conductor; the mass percentage of each component in the composite solid electrolyte is: 25% to 90% of the polymer matrix, 1% to 70% of the inorganic filler; the molar ratio of the sodium salt to the polymer monomer is (0.1 to 1): 20, which will not be repeated here. It can be understood that in some other embodiments, the content of each component raw material added in the above preparation method can also be appropriately adjusted according to demand.

[0058] Specifically, in this embodiment, the first organic solvent, the second organic solvent or the third organic solvent is one or a combination of acetone, DMF and NMP.

[0059] Among them, the mass percentage of the second organic solvent in the composite negative electrode slurry is 50% to 80%. It can be understood that the mass percentage of the second organic solvent in the composite negative electrode slurry can be 50%, 55%, 60%, 65%, 70%, 75%, 80%, or other percentages within the above range. The mass percentage of the third organic solvent in the composite positive electrode slurry is 50% to 80%. It can be understood that the mass percentage of the third organic solvent in the composite positive electrode slurry can be 50%, 55%, 60%, 65%, 70%, 75%, 80%, or other percentages within the above range. The mass percentage of the first organic solvent in the composite solid electrolyte slurry is 67% to 83%. It can be understood that the mass percentage of the first organic solvent to the mass percentage of the composite solid electrolyte slurry can be 67%, 70%, 72%, 75%, 77%, 78%, 80%, 81%, 82%, 83%, or other percentages within the above range.

[0060] In order to obtain a uniform composite negative electrode slurry, in step S3, the negative electrode active material, the second binder, the second conductive agent, the second organic solvent and the second sodium ion conductor are mixed, and then the composite negative electrode slurry is obtained by magnetic stirring for 6 hours to 18 hours. It can be understood that the magnetic stirring time can be 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 15 hours, 17 hours, 18 hours, or other time values ​​within the above range.

[0061] In order to obtain a uniform composite solid electrolyte slurry, in step S1, after mixing the polymer matrix, the inorganic filler, the sodium salt and the first organic solvent, the composite solid electrolyte slurry is obtained by magnetic stirring for 6 hours to 18 hours. It can be understood that the magnetic stirring time can be 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 15 hours, 17 hours, 18 hours, or other time values ​​within the above range.

[0062] In order to obtain a uniform composite positive electrode slurry, in step S5, the positive electrode active material, the first binder, the first conductive agent, the third organic solvent and the first sodium ion conductor are mixed, and then the composite positive electrode slurry is obtained by magnetic stirring for 6 hours to 18 hours. It can be understood that the magnetic stirring time can be 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 15 hours, 17 hours, 18 hours, or other time values ​​within the above range.

[0063] In order to obtain an integrated battery cell with good electrochemical performance and mechanical strength, in step S2, the coating thickness of the composite solid electrolyte slurry is 80 μm to 300 μm. It can be understood that the coating thickness of the composite solid electrolyte slurry can be 80 μm, 90 μm, 100 μm, 120 μm, 150 μm, 180 μm, 200 μm, 240 μm, 260 μm, 280 μm, 300 μm, or other coating thickness values ​​within the above range.

[0064] In order to ensure the excellent performance of the obtained electrode and solid electrolyte integrated battery cell, such as battery capacity, charge and discharge efficiency and cycle life, in step S4, the coating thickness of the composite negative electrode layer is 10μm to 80μm; in step S6, the coating thickness of the composite positive electrode layer is 10μm to 80μm. It can be understood that the coating thickness of the composite negative electrode layer can be 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, or other coating thickness values ​​within the above range; the coating thickness of the composite positive electrode layer can be 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, or other coating thickness values ​​within the above range.

[0065] In order to obtain the composite solid electrolyte film with excellent performance, in step S2, after the composite solid electrolyte slurry is coated on the polytetrafluoroethylene mold, the temperature of the blast drying is 25°C to 80°C, and the drying time is 5min to 30min. It can be understood that the temperature of the blast drying can be 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, or other blast drying temperature values ​​within the above range; the drying time can be 30min, 27min, 23min, 19min, 15min, 14min, 12min, 11min, 9min, 7min, 6min, 5min, or other drying time values ​​within the above range. In this embodiment, the temperature of the blast drying is 45°C and the drying time is 15min.

[0066] In order to obtain the performance of the laminated structure of the composite negative electrode layer and the composite solid electrolyte, in step S4, after the composite negative electrode slurry is coated on the composite solid electrolyte, the temperature of the blast drying is 25°C to 80°C, and the drying time is 5min to 30min. It can be understood that the temperature of the blast drying can be 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, or other blast drying temperature values ​​within the above range; the drying time can be 30min, 27min, 23min, 19min, 15min, 14min, 12min, 10min, 9min, 7min, 6min, 5min, or other drying time values ​​within the above range. In this embodiment, the temperature of the blast drying is 60°C and the drying time is 10min.

[0067] In order to obtain the electrode and solid electrolyte integrated battery cell required by the present invention, in step S6, after the composite positive electrode slurry is coated on the side of the composite solid electrolyte in the laminated structure obtained in step S4 away from the composite negative electrode layer, the air drying temperature is 25°C to 80°C, and the air drying time is 30min to 120min; the vacuum drying temperature is 45°C to 80°C, and the vacuum drying time is 12h to 36h. It can be understood that the temperature of blast drying can be 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, or other blast drying temperature values ​​within the above range; the blast drying time can be 120min, 115min, 110min, 100min, 95min, 90min, 85min, 80min, 65min, 50min, 38min, 30min, or other blast drying time within the above range; the temperature of vacuum drying can be 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, or other vacuum drying temperature values ​​within the above range; the vacuum drying time can be 36h, 34h, 31h, 28h, 24h, 18h, 15h, 12h, or other vacuum drying time values ​​within the above range. In this embodiment, the temperature of blast drying is 60° C., the time of blast drying is 80 min, the temperature of vacuum drying is 65° C., and the time of vacuum drying is 24 h.

[0068] In another aspect, the embodiments of the present invention further provide a solid-state sodium ion battery. The solid-state sodium ion battery in this embodiment comprises the electrode and solid electrolyte integrated battery cell described in any of the above embodiments or the electrode and solid electrolyte integrated battery cell prepared by the preparation method.

[0069] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with specific examples, but the content of the present invention is not limited to the following examples.

[0070] Example 1

[0071] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 0.83 g PVDF-HFP, 0.27 g diethyl phthalate, 0.091 g NaFSI and 5.5 g DMF were mixed and magnetically stirred for 8 h to obtain a transparent solution; 0.83 g Na3Zr2Si2PO 12 The powder was added into the above solution and magnetically stirred for 18 h to obtain a composite solid electrolyte slurry.

[0072] Step 2: Take the composite solid electrolyte slurry obtained in step 1 out of the glove box, apply it on a polytetrafluoroethylene mold with a scraper height of 0.5 mm, and blow dry it to obtain a composite solid electrolyte film.

[0073] Step 3: In a glove box, 0.35 g of hard carbon (Kuraray), 0.05 g of PVDF, 0.05 g of acetylene black, 0.05 g of SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) and 1.58 g of NMP were mixed and magnetically stirred for 12 h to obtain a composite negative electrode slurry.

[0074] Step 4: The composite negative electrode slurry obtained in step 3 is coated on the composite solid electrolyte body obtained in step 2 with a thickness of 0.04 mm, and air-dried to obtain a laminated structure of a composite negative electrode layer and a composite solid electrolyte.

[0075] Step 5: In a glove box, take 0.35g Na3V2(PO4)3, 0.05g PVDF, 0.05g acetylene black, 0.05g SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) and mix with 1.58g NMP, and stir magnetically for 12h to obtain a composite positive electrode slurry.

[0076] Step six: Apply the composite positive electrode slurry obtained in the above step five with a thickness of 0.04 mm on the side of the composite solid electrolyte of the laminated structure obtained in the above step four away from the composite negative electrode layer, blow dry at 60°C for 1 hour, and then dry in a vacuum environment at 60°C for 24 hours to obtain an electrode and composite solid electrolyte integrated battery cell.

[0077] See also Figure 2 , Figure 2 The cross-sectional SEM image of the electrode and solid electrolyte integrated battery cell prepared by the above preparation method is shown. Figure 2The characterization results show that the electrode and solid electrolyte integrated battery cell prepared by the above preparation method has a uniform planar structure and the layers are strongly bonded and do not separate.

[0078] In this embodiment, the electrode and solid electrolyte integrated battery cell prepared by the above preparation method is cut into φ16mm discs and assembled into CR2032 button batteries. The CR2032 button batteries are C|SEs (solid electrolyte)|Na3V2(PO4)3 batteries, and the impedance of this battery is 1196.9Ω.

[0079] See also Figure 3 , Figure 3 The impedance data of the C|SEs|Na3V2(PO4)3 battery of this embodiment is shown. It can be clearly seen from the figure that the battery impedance obtained in this embodiment is small, so a higher transmission efficiency of sodium ions can be achieved.

[0080] The above batteries were tested for charge and discharge performance at 0.1C, 0.1~3V and 55℃. Figure 5 , Figure 5 The charge and discharge cycle performance of the C|SEs|Na3V2(PO4)3 battery in Example 1 is shown. It can be seen that the battery has a high specific capacity and good specific capacity stability. Its specific capacity fluctuation is extremely small within a certain number of cycles; the charge and discharge efficiency has good stability within a certain number of cycles.

[0081] Example 2

[0082] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 0.72 g PVDF-HFP, 0.135 g PEG, 0.035 g NaClO4 and 5.5 g DMF were mixed and magnetically stirred for 3 h to obtain a transparent solution; 0.62 g Na3Zr2Si2PO 12 The powder was added into the above solution and magnetically stirred for 18 h to obtain a composite solid electrolyte slurry.

[0083] Step 2: Take the composite solid electrolyte slurry obtained in step 1 out of the glove box, apply it on a polytetrafluoroethylene mold with a scraper height of 0.5 mm, and dry it with air to obtain a composite solid electrolyte film. Step 3:

[0084] In a glove box, 0.35 g Na2Ti3O7, 0.05 g PVDF-HFP, 0.05 g acetylene black, 0.05 g SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) were mixed with 1.58 g NMP and magnetically stirred for 12 h to obtain a composite negative electrode slurry.

[0085] Step 4: The composite negative electrode slurry obtained in step 3 is coated on the composite solid electrolyte body obtained in step 2 with a thickness of 0.04 mm, and air-dried to obtain a laminated structure of a composite negative electrode layer and a composite solid electrolyte.

[0086] Step 5: In a glove box, 0.35 g Na3V2(PO4)3, 0.05 g PVDF-HFP, 0.05 g acetylene black, 0.05 g SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) and 1.58 g NMP were mixed and magnetically stirred for 12 h to obtain a composite positive electrode slurry.

[0087] Step six: Apply the composite positive electrode slurry obtained in the above step five with a thickness of 0.04 mm on the side of the composite solid electrolyte of the laminated structure obtained in the above step four away from the composite negative electrode layer, blow dry at 60°C for 1 hour, and then dry in a vacuum environment at 60°C for 24 hours to obtain an electrode and composite solid electrolyte integrated battery cell.

[0088] In this embodiment, the electrode and solid electrolyte integrated battery cell prepared by the above preparation method is cut into φ16mm discs and assembled into CR2032 button batteries. The CR2032 button batteries are Na2Ti3O7|SEs|Na3V2(PO4)3 batteries, and the battery impedance is 1243.2Ω.

[0089] See also Figure 3 , Figure 3 The impedance data of the Na2Ti3O7|SEs|Na3V2(PO4)3 battery of this embodiment is shown. It can be clearly seen from the figure that the battery impedance obtained in this embodiment is small, so a higher transmission efficiency of sodium ions can be achieved.

[0090] The above batteries were tested for charge and discharge performance at 0.1C, 0.1~3V and 55℃. Figure 5 , Figure 5 The charge and discharge performance of the Na2Ti3O7|SEs|Na3V2(PO4)3 battery of this embodiment is shown. It can be seen that the battery has a high specific capacity and charge and discharge efficiency, and the specific capacity and charge and discharge efficiency gradually tend to be stable with the increase of the number of cycles. The stability is good within the number of cycles, and thus the battery has a good service life.

[0091] Example 3

[0092] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 0.80 g PEO, 0.27 g SN, 0.07 g NaClO4 and 5.5 g NMP were mixed and magnetically stirred for 3 h to obtain a transparent solution; 0.72 g Na3Zr2Si2PO 12The powder was added into the above solution and magnetically stirred for 18 h to obtain a composite solid electrolyte slurry.

[0093] Step 2: Take the composite solid electrolyte slurry obtained in step 1 out of the glove box, apply it on a polytetrafluoroethylene mold with a scraper height of 0.5 mm, and blow dry to obtain a composite solid electrolyte film. Step 3: Take 0.35g hard carbon (Kuraray), 0.05g PEO, 0.05g acetylene black, 0.05g SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) and 1.58g NMP in the glove box, mix them, and stir them magnetically for 12h to obtain a composite negative electrode slurry.

[0094] Step 4: The composite negative electrode slurry obtained in step 3 is coated on the composite solid electrolyte body obtained in step 2 with a thickness of 0.04 mm, and air-dried to obtain a laminated structure of a composite negative electrode layer and a composite solid electrolyte.

[0095] Step 5: In a glove box, take 0.35g Na3V2(PO4)3, 0.05g PEO, 0.05g acetylene black, 0.05g SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) and mix with 1.58g NMP, and stir magnetically for 12h to obtain a composite positive electrode slurry.

[0096] Step six: Apply the composite positive electrode slurry obtained in the above step five with a thickness of 0.04 mm on the side of the composite solid electrolyte of the laminated structure obtained in the above step four away from the composite negative electrode layer, blow dry at 60°C for 1 hour, and then dry in a vacuum environment at 60°C for 24 hours to obtain an electrode and composite solid electrolyte integrated battery cell.

[0097] In this embodiment, the electrode and solid electrolyte integrated battery cell prepared by the above preparation method is cut into φ16mm discs and assembled into CR2032 button batteries. The CR2032 button batteries are C|SEs|Na3V2(PO4)3 batteries, and the battery impedance is 987.1Ω.

[0098] See also Figure 3 , Figure 3 The impedance data of the C|SEs|Na3V2(PO4)3 battery of this embodiment is shown. It can be clearly seen from the figure that the battery impedance obtained in this embodiment is small, so a higher transmission efficiency of sodium ions can be achieved.

[0099] The above batteries were tested for charge and discharge performance at 0.1C, 0.1~3V and 55℃. Figure 6 , Figure 6The charge and discharge performance of the C|SEs|Na3V2(PO4)3 battery of this embodiment is shown. It can be seen that the battery has a high specific capacity and charge and discharge efficiency within the number of cycles in the test, and the specific capacity performance and charge and discharge efficiency are stable during the cycle process, so it has a good service life.

[0100] Example 4

[0101] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 0.91 g PVDF-HFP, 0.27 g SN, 0.07 g NaClO4, 3.5 g DMF and 2 g NMP were mixed and magnetically stirred for 3 h to obtain a transparent solution; 0.71 g Na 3.4 Zr 1.8 Mg 0.2 Si2PO 12 The powder was added into the above solution and magnetically stirred for 18 h to obtain a composite solid electrolyte slurry.

[0102] Step 2: Take the composite solid electrolyte slurry obtained in step 1 out of the glove box, apply it on a polytetrafluoroethylene mold with a scraper height of 0.5 mm, and blow dry it to obtain a composite solid electrolyte film.

[0103] Step 3: In a glove box, 0.35 g of hard carbon (Kuraray), 0.05 g of PVDF-HFP, 0.05 g of acetylene black, 0.025 g of SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) and 1.58 g of NMP were mixed and magnetically stirred for 12 h to obtain a composite negative electrode slurry.

[0104] Step 4: The composite negative electrode slurry obtained in step 3 is coated on the composite solid electrolyte body obtained in step 2 with a thickness of 0.04 mm, and air-dried to obtain a laminated structure of a composite negative electrode layer and a composite solid electrolyte.

[0105] Step 5: In a glove box, take 0.35g Na3V2(PO4)3, 0.05g PVDF-HFP, 0.05g acetylene black, 0.025g SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) and mix with 1.58g NMP, and stir magnetically for 12h to obtain a composite positive electrode slurry.

[0106] Step six: Apply the composite positive electrode slurry obtained in the above step five with a thickness of 0.04 mm on the side of the composite solid electrolyte of the laminated structure obtained in the above step four away from the composite negative electrode layer, blow dry at 60°C for 1 hour, and then dry in a vacuum environment at 60°C for 24 hours to obtain an electrode and composite solid electrolyte integrated battery cell.

[0107] In this embodiment, the electrode and solid electrolyte integrated battery cell prepared by the above preparation method is cut into φ16mm discs and assembled into CR2032 button batteries. The CR2032 button batteries are C|SEs|Na3V2(PO4)3 batteries, and the battery impedance is 1007.5Ω.

[0108] See also Figure 4 , Figure 4 The impedance data of the C|SEs|Na3V2(PO4)3 battery of this embodiment is shown. It can be clearly seen from the figure that the battery impedance obtained in this embodiment is small, so a high transmission efficiency of sodium ions can be achieved, indicating that the battery has good electrochemical performance.

[0109] The above batteries were tested for charge and discharge performance at 0.1C, 0.1~3V and 55℃. Figure 6 , Figure 6 The charge and discharge performance of the C|SEs|Na3V2(PO4)3 battery of this embodiment is shown. It can be seen that the battery has a high specific capacity and charge and discharge efficiency within the number of cycles in this test, and the specific capacity performance and charge and discharge efficiency are stable during the cycle process, so it has a good service life.

[0110] Example 5

[0111] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 0.71 g PVDF-HFP, 0.27 g SN, 0.096 g NaFSI and 5.5 g DMF were mixed and magnetically stirred for 3 h to obtain a transparent solution; 0.54 g Na3Zr2Si2PO 12 The powder was added into the above solution and magnetically stirred for 18 h to obtain a composite solid electrolyte slurry.

[0112] Step 2: Take the composite solid electrolyte slurry obtained in step 1 out of the glove box, apply it on a polytetrafluoroethylene mold with a scraper height of 0.5 mm, and blow dry it to obtain a composite solid electrolyte film.

[0113] Step 3: In a glove box, 0.35 g of hard carbon (Kuraray), 0.05 g of PVDF-HFP, 0.05 g of carbon nanotubes, 0.05 g of SN-NaCOl4 (the molar ratio of sodium ions to SN is 1:20) and 1.58 g of NMP were mixed and magnetically stirred for 12 h to obtain a composite negative electrode slurry.

[0114] Step 4: The composite negative electrode slurry obtained in step 3 is coated on the composite solid electrolyte body obtained in step 2 with a thickness of 0.04 mm, and air-dried to obtain a laminated structure of a composite negative electrode layer and a composite solid electrolyte.

[0115] Step 5: In a glove box, take 0.35 g Na3V2(PO4)3, 0.05 g PVDF-HFP, 0.05 g carbon nanotubes, 0.05 g SN-NaCOl4 (the molar ratio of sodium ions to SN is 1:20) and mix with 1.58 g NMP, and stir magnetically for 12 h to obtain a composite positive electrode slurry.

[0116] Step six: Apply the composite positive electrode slurry obtained in the above step five with a thickness of 0.04 mm on the side of the composite solid electrolyte of the laminated structure obtained in the above step four away from the composite negative electrode layer, blow dry at 60°C for 1 hour, and then dry in a vacuum environment at 60°C for 24 hours to obtain an electrode and composite solid electrolyte integrated battery cell.

[0117] In this embodiment, the electrode and solid electrolyte integrated battery cell prepared by the above preparation method is cut into φ16mm discs and assembled into CR2032 button batteries. The CR2032 button batteries are C|SEs|Na3V2(PO4)3 batteries, and the battery impedance is 1226.5Ω.

[0118] See also Figure 4 , Figure 4 The impedance data of the C|SEs|Na3V2(PO4)3 battery of this embodiment is shown. It can be clearly seen from the figure that the battery impedance obtained in this embodiment is small, so a higher transmission efficiency of sodium ions can be achieved.

[0119] Comparative Example 1

[0120] Step 1: In a glove box with an argon atmosphere and water content ≤ 0.1 ppm, 0.51 g PVDF-HFP, 0.135 g PEG, 0.07 g NaClO4 and 5.5 g DMF were mixed and magnetically stirred for 3 h to obtain a transparent solution; 0.62 g Na3Zr2Si2PO 12 The powder was added into the above solution and magnetically stirred for 18 h to obtain a composite solid electrolyte slurry.

[0121] Step 2: The composite solid electrolyte slurry obtained in the above step 1 is coated on a polytetrafluoroethylene template with a thickness of 0.5 mm, and dried at 45° C. for 2 h and vacuum dried at 60° C. for 24 h to obtain a composite solid electrolyte membrane.

[0122] Step 3: In a glove box, 0.35 g of hard carbon (Kuraray), 0.05 g of PVDF, 0.05 g of acetylene black, 0.05 g of SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) and 1.58 g of NMP were mixed and magnetically stirred for 12 h to obtain a composite negative electrode slurry.

[0123] Step 4: Take out the composite negative electrode slurry obtained in the above step 3 from the glove box, apply the slurry on copper foil with a thickness of 0.04 mm, dry it at 60° C. for 1 h, and then dry it at 60° C. in vacuum for 24 h to obtain a composite negative electrode layer.

[0124] Step 5: In a glove box, take 0.35g Na3V2(PO4)3, 0.05g PVDF, 0.05g acetylene black, 0.05g SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) and mix with 1.58g NMP, and stir magnetically for 12h to obtain a composite positive electrode slurry.

[0125] Step 6: Similarly, the composite positive electrode slurry obtained in the above step 5 is coated on an aluminum foil with a thickness of 0.04 mm, dried at 60° C. for 1 h, and then vacuum dried at 60° C. for 24 h to obtain a composite positive electrode layer.

[0126] In this comparative example, the composite negative electrode layer obtained in the above step 4 and the composite positive electrode layer in step 6 were cut into φ16 mm round pieces, and the composite solid electrolyte membrane obtained in step 2 was cut into φ19 mm round pieces, and assembled with a copper current collector into a CR2032 button-type solid-state sodium ion battery.

[0127] After being kept at 80℃ for 2h, the performance test was carried out, and the impedance of the C|SEs|Na3V2(PO4)3 battery obtained in this comparative example was 4492.7Ω. Figure 3 , Figure 3 The impedance data of the comparative example C|SEs|Na3V2(PO4)3 battery is shown.

[0128] The battery obtained in this comparative example was tested for charge and discharge performance at 0.1C, 0.1-3V and 55°C. Figure 5 , Figure 5 The charge and discharge performance of the comparative example C|SEs|Na3V2(PO4)3 battery is shown.

[0129] Comparative Example 2

[0130] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 0.81 g PVDF-HFP, 0.135 g PEG, 0.1 g NaFSI and 5.5 g DMF were mixed and magnetically stirred for 3 h to obtain a transparent solution; 0.53 g Na3Zr2Si2PO 12 The powder was added into the above solution and magnetically stirred at 45° C. for 18 h to obtain a composite solid electrolyte slurry.

[0131] Step 2: The composite solid electrolyte slurry obtained in the above step 1 is coated on a polytetrafluoroethylene template with a thickness of 0.5 mm, and dried at 45° C. for 2 h and vacuum dried at 60° C. for 24 h to obtain a composite solid electrolyte membrane.

[0132] Step 3: In a glove box, take 0.35g Na2Ti3O7, 0.05g PVDF-HFP, 0.05g acetylene black, 0.05g SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) and mix with 1.58g NMP, and stir magnetically for 12h to obtain a composite negative electrode slurry.

[0133] Step 4: Take the composite negative electrode slurry obtained in the above step 3 out of the glove box, apply the slurry on the copper foil with a thickness of 0.04 mm, dry it at 60°C for 1 hour, and then vacuum dry it at 60°C for 24 hours to obtain a composite negative electrode layer. Step 5: Take 0.35g Na3V2(PO4)3, 0.05g PVDF-HFP, 0.05g acetylene black, 0.05g SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) and 1.58g NMP in the glove box, mix them, and stir them magnetically for 12 hours to obtain a composite positive electrode slurry.

[0134] Step 6: The composite positive electrode slurry obtained in the above step 5 is coated on an aluminum foil with a thickness of 0.04 mm, dried at 60° C. for 1 h, and then vacuum dried at 60° C. for 24 h to obtain a composite positive electrode layer.

[0135] In this comparative example, the composite negative electrode layer obtained in step 4 and the composite positive electrode layer in step 6 were cut into φ16mm discs, and the composite solid electrolyte membrane obtained in step 2 was cut into φ19mm discs, and assembled with the copper current collector into a CR2032 button-type solid-state sodium ion battery. The battery was subjected to performance testing after being kept at 80°C for 2h. The battery impedance obtained in this comparative example was 4326.4Ω. Please refer to Figure 4 , Figure 4 The impedance data of the comparative example Na2Ti3O7|SEs|Na3V2(PO4)3 battery is shown.

[0136] The battery obtained in this comparative example was tested for charge and discharge performance at 0.1C, 0.1-3V and 55°C. Figure 6 , Figure 6 The charging and power generation performance of the comparative example Na2Ti3O7|SEs|Na3V2(PO4)3 battery is shown.

[0137] Comparative Example 3

[0138] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 8.1 g PEO, 0.27 g SN, 0.07 g NaClO4 and 5.5 g DMF were mixed and magnetically stirred for 3 h to obtain a transparent solution; 0.72 g Na3Zr2Si2PO 12 The powder was added into the above solution and magnetically stirred for 18 h to obtain a composite solid electrolyte slurry.

[0139] Step 2: The composite solid electrolyte slurry obtained in the above step 1 is coated on a polytetrafluoroethylene template with a thickness of 0.5 mm, and dried at 45° C. for 2 h and vacuum dried at 60° C. for 24 h to obtain a composite solid electrolyte membrane.

[0140] Step 3: In a glove box, 0.35 g of hard carbon (Kuraray), 0.05 g of PEO, 0.05 g of acetylene black, 0.025 g of SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) and 1.58 g of NMP were mixed and magnetically stirred for 12 h to obtain a composite negative electrode slurry.

[0141] Step 4: Take out the composite negative electrode slurry obtained in the above step 3 from the glove box, apply the slurry on copper foil with a thickness of 0.04 mm, dry it at 60° C. for 1 h, and then dry it at 60° C. in vacuum for 24 h to obtain a composite negative electrode layer.

[0142] Step 5: In a glove box, take 0.35g Na3V2(PO4)3, 0.05g PEO, 0.05g acetylene black, 0.025g SN-NaCOl4 (the molar ratio of sodium ion to SN is 1:20) and mix with 1.58g NMP, and stir magnetically for 12h to obtain a composite positive electrode slurry.

[0143] Step 6: The composite positive electrode slurry obtained in the above step 5 is coated on an aluminum foil with a thickness of 0.04 mm, dried at 60° C. for 1 h, and then vacuum dried at 60° C. for 24 h to obtain a composite positive electrode layer.

[0144] In this comparative example, the composite negative electrode layer obtained in the above step 4 and the composite positive electrode layer in step 6 were cut into φ16 mm round pieces, and the composite solid electrolyte membrane obtained in step 2 was cut into φ19 mm round pieces, and assembled with a copper current collector into a CR2032 button-type solid-state sodium ion battery.

[0145] The battery was kept at 80°C for 2 hours before the performance test was conducted. The test showed that the battery impedance obtained in this comparative example was 4412.1Ω. Figure 4 , Figure 4 The impedance data of the comparative example C|SEs|Na3V2(PO4)3 battery is shown.

[0146] Table 1 shows the electrochemical impedance data and charge-discharge efficiency of the batteries of Examples 1 to 5 and Comparative Examples 1 to 3. As can be seen from Table 1, the charge-discharge efficiency of the electrode and solid electrolyte integrated battery cell (CR2032 button type) prepared by the present invention is significantly higher than that of the non-integrated solid battery cell, and the electrochemical impedance of the integrated solid battery cell (CR2032 button type) is significantly lower than that of the non-integrated solid battery cell. This indicates that the electrode and solid electrolyte of the electrode and solid electrolyte integrated battery cell prepared by the present invention are in close contact with the solid electrolyte and have a low interface impedance, which can facilitate the rapid transmission of sodium ions at the interface.

[0147] Table 1 Electrochemical impedance data of solid-state sodium ion battery

[0148] project Electrochemical impedance (Ω) Charge and discharge efficiency (%) Example 1 1196.9 99.7% Example 2 1243.2 99.7% Example 3 987.1 99.8% Example 4 1007.5 99.6% Example 5 1226.5 99.5% Comparative Example 1 4492.7 99.2% Comparative Example 2 4326.4 99.2% Comparative Example 3 4412.1 993%

[0149] Figure 3 The electrochemical impedance diagrams of the sodium ion batteries of Example 1, Example 2, Example 3 and Comparative Example 1 of the present invention are shown, wherein □ represents a point on the curve of Example 1, ◇ represents a point on the curve of Example 2, △ represents a point on the curve of Example 3, and ○ represents a point on the curve of Comparative Example 1. Figure 4 The electrochemical impedance diagrams of sodium ion batteries of Example 4, Example 5, Comparative Example 2 and Comparative Example 3 are shown, where ▽ represents a point on the curve of Example 4, ○ represents a point on the curve of Example 5, △ represents a point on the curve of Comparative Example 2, and ◇ represents a point on the curve of Comparative Example 3. Figure 3 and Figure 4 It can be seen that the electrochemical impedance of the sodium ion battery corresponding to the electrode and solid electrolyte integrated battery cell is smaller than the electrochemical impedance of the non-integrated battery.

[0150] Figure 5 The charge and discharge cycle curves of sodium ion batteries (CR2032 button type) of Example 1, Example 2 and Comparative Example 1 of the present invention are shown. □ represents a point on the discharge specific capacity curve of Example 1, △ represents a point on the discharge specific capacity curve of Example 2, and ▽ represents a point on the discharge specific capacity curve of Comparative Example 1; ☆ represents a point on the efficiency curve of Example 1, ○ represents a point on the efficiency curve of Example 2, and × represents a point on the efficiency curve of Comparative Example 1. Figure 6 The charge and discharge cycle curves of sodium ion batteries (CR2032 button type) of Example 3, Example 4 and Comparative Example 2 of the present invention are shown. □ represents a point on the discharge capacity curve of Example 3, ◇ represents a point on the discharge capacity curve of Example 4, and ▽ represents a point on the discharge capacity curve of Comparative Example 2; ○ represents a point on the efficiency curve of Example 3, △ represents a point on the efficiency curve of Example 4, and × represents a point on the efficiency curve of Comparative Example 2. Figure 5 and Figure 6 It can be seen that the sodium ion battery corresponding to the integrated electrode and solid electrolyte cell has better charging and discharging performance.

[0151] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. An electrode and solid electrolyte integrated battery cell, characterized in that: The invention comprises a composite positive electrode layer and a composite negative electrode layer, and a composite solid electrolyte arranged between the composite negative electrode layer and the composite positive electrode layer, wherein The composite positive electrode layer comprises a positive electrode active material, a first binder, a first conductive agent and a first sodium ion conductor material; The composite negative electrode layer comprises a negative electrode active material, a second binder, a second conductive agent and a second sodium ion conductor material; The composite solid electrolyte comprises a polymer matrix, an inorganic filler and a sodium salt.

2. The electrode and solid electrolyte integrated battery cell according to claim 1, characterized in that: The mass percentage of each component in the composite negative electrode layer is: 30% to 80% of the negative electrode active material, 1% to 20% of the second binder, 1% to 20% of the second conductive agent, and 1% to 20% of the second sodium ion conductor.

3. The electrode and solid electrolyte integrated battery cell according to claim 1, characterized in that: The mass percentage of each component in the composite positive electrode layer is: 30% to 80% of the positive electrode active material, 1% to 20% of the first binder, 1% to 20% of the first conductive agent, and 1% to 20% of the first sodium ion conductor.

4. The electrode and solid electrolyte integrated battery cell according to claim 1, characterized in that: The mass percentage of each component in the composite solid electrolyte is: 25% to 90% of the polymer matrix, 1% to 70% of the inorganic filler; the molar ratio of the sodium salt to the polymer monomer is (0.1 to 1):

20.

5. The electrode and solid electrolyte integrated battery cell according to claim 1, 2 or 3, characterized in that: The positive electrode active material is selected from Na 1-x FeO2、Na 1-x [Fe 1-x Mn x ]O2(x≤0.5),Na 1-x CoO2、Na 0.7 [(Fe 0.5 Mn 0.5 ) 1-x Co x ]O2、Na x MnO2、Na 2 / 3 [Co 1-x Mn x ]O2、Na 2 / 3x Ca x CoO2、Na 1-x NiO2, Na[Ni 0.75x Fe x Mn 0.25 ]O2、Na 1-x TiO2、Na 1- x CrO2、Na 1-x VO2、Na 2 / 3 [Ni 1 / 3x Mg x Mn 0.7 ]O2、Na 2 / 3 [Ni 1 / 3x Zn x Mn 2 / 3 ]O2、Na 2 / 3 [Ni 1 / 3 Mn 2 / 3x Ti x ]O2、Na 1- x FePO4, Na3V2(PO4)3, Na x [Fe 0.5 Mn 0.5 ]PO4、Na 2-x FePO4F 1-y 、NaVPO4F 1-x 、Na3Fe2(PO4)2F 3-x , at least one of Na4M3(PO4)2P2O7 (M: Mn, Fe, Co, Ni), NaMSO4F (M: Fe, Co, Mn), Na3MPO4CO3 (M: Mg, Mn, Fe, Co, Ni, Cu), Prussian blue, and Prussian white; The negative electrode active material is selected from hard carbon, graphite, TiO2, Li4Ti5O 12 、LiNa6Ti5O 12 、Li7Ti5O 12 、Na 3–x Ti3O7、Na 2+x Ti6O 13 , NiCo2O4, SnO, SnO2, CuO, MS (M: Mn, Fe, Co, Ti, Cu, Sn, Mo, W), MS2 (M: Mn, Fe, Co, Ti, Cu, Sn, Mo, W), MP (M: Ni, Fe, Co, Cu, Sn); The first binder and the second binder are both selected from at least one of polyethylene oxide (PEO), polyacrylonitrile (PAN), poly(methyl methacrylate) (PMMA), poly(vinyl alcohol) (PVA), polyvinyl pyrrolidone (PVP), polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), polypropylene carbonate (PPC), and polyethylene carbonate (PEC); The first conductive agent and the second conductive agent are both selected from at least one of graphite, graphene, carbon nanotubes, and acetylene black; The first sodium ion conductor and the second sodium ion conductor are both selected from Na 1+x Zr2Si x P 3-x O 12 (0≤x≤3), NaMM′P3O 12 (M and M' are Si 2+ ,Mg 2+ , Cu 2+ ,Co 2+ , Zn 2+ , Mn 2+ , Fe 2+ , Al 3+ ,Cr 3+ , Sc 3+ , Y 3+ , La 3+ , Ti 4+ , Zr 4+ ,Ge 4+ , Sn 4+ , Nb 4+ , V 5+ , Nb 5+ , 5+ the same element or different elements), β″-Al2O3, β-Al2O3, Na3PS4, Na3SbS4, Na 11 Sn2PS 12 、Na4Sn 0.67 Si 0.33 S4, at least one of a succinonitrile-NaClO4 complex.

6. The electrode and solid electrolyte integrated battery cell according to claim 1 or 4, characterized in that: The polymer matrix is ​​selected from at least one of PEO, PAN, PMMA, PVA, PVP, PVDF, PVDF-HFP, PPC, PEC, succinonitrile (SN), and polyethylene glycol (PEG); The inorganic filler is selected from Si, AlCl3, BaTiO3, CuO, SiO2, ZrO2, TiO2, Na 1+x Zr2Si x P 3-x O 12 (0≤x≤3), NaMM′P3O 12 (M and M' are Si 2+ ,Mg 2+ , Cu 2+ ,Co 2+ , Zn 2+ , Mn 2+ , Fe 2+ , Al 3+ ,Cr 3+ , Sc 3+ , Y 3+ , La 3+ , Ti 4+ , Zr 4+ ,Ge 4+ , Sn 4+ , Nb 4+ , V 5+ , Nb 5+ , 5+ the same element or different elements), β″-Al2O3, β-Al2O3, Na3PS4, Na3SbS4, Na 11 Sn2PS 12 、Na4Sn 0.67 Si 0.33 At least one of S4; The sodium salt is selected from at least one of NaClO4, NaPF6, NaAsF6, NaBF4, NaTFSI, NaTf, NaFSI, and sodium bis(oxalate)borate.

7. A method for preparing an electrode and solid electrolyte integrated battery cell, characterized in that: The following steps are involved: Mixing a polymer matrix, an inorganic filler, a sodium salt and a first organic solvent to obtain a composite solid electrolyte slurry; The composite solid electrolyte slurry is coated on a polytetrafluoroethylene mold and dried with air blast to obtain a composite solid electrolyte film; Mixing the negative electrode active material, the second binder, the second conductive agent, the second organic solvent and the second sodium ion conductor to obtain a composite negative electrode slurry; The composite negative electrode slurry is coated on the composite solid electrolyte film and dried by air blast to obtain a laminated structure of a composite negative electrode layer and a composite solid electrolyte; The positive electrode active material, the first binder, the first conductive agent, the third organic solvent and the first sodium ion conductor are mixed to obtain a composite positive electrode slurry; The composite positive electrode slurry is coated on a side of the composite solid electrolyte film away from the composite negative electrode layer, and then air-dried and vacuum-dried to obtain an electrode and solid electrolyte integrated battery cell.

8. The method for preparing an electrode and solid electrolyte integrated battery cell according to claim 7, characterized in that: The first organic solvent, the second organic solvent or the third organic solvent includes one or a combination of acetone, N,N-dimethylformamide (DMF) and nitrogen methyl pyrrolidone (NMP).

9. The method for preparing an electrode and solid electrolyte integrated battery cell according to claim 7, characterized in that: The mass percentage of each component in the composite negative electrode layer is: 30% to 80% of the negative electrode active material, 1% to 20% of the second binder, 1% to 20% of the second conductive agent, and 1% to 20% of the second sodium ion conductor; the mass percentage of each component in the composite positive electrode layer is: 30% to 80% of the positive electrode active material, 1% to 20% of the first binder, 1% to 20% of the first conductive agent, and 1% to 20% of the first sodium ion conductor; the mass percentage of each component in the composite solid electrolyte is: 25% to 90% of the polymer matrix, and 1% to 70% of the inorganic filler; the molar ratio of the sodium salt to the polymer monomer is (0.1 to 1):

20.

10. A solid-state sodium ion battery, characterized in that: It comprises the electrode and solid electrolyte integrated battery cell as described in any one of claims 1 to 6, or the electrode and solid electrolyte integrated battery cell prepared by the preparation method as described in any one of claims 7 to 9.