Light-emitting device, display screen, electronic equipment and preparation method of light-emitting device

By arranging a stacked structure of hole transport layers in the light-emitting device of the AMOLED display, the mobility of hole carriers is improved, the problem of color deviation of the light-emitting device is solved, and the stability of the device and user experience are improved.

CN118829263APending Publication Date: 2024-10-22BEIJING XIAOMI MOBILE SOFTWARE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310414498.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

When the light-emitting devices of existing AMOLED displays work for a long time, the hole carrier migration efficiency of the hole transport layer decreases, resulting in color deviation and affecting the user experience.

Method used

A light-emitting device is designed, including a hole injection layer, a hole transport layer and a light-emitting layer arranged in a stack. The hole transport layer is composed of a first transport layer, a second transport layer and a third transport layer. The third transport layer The hole mobility is greater than that of the second transport layer. The hole mobility of the second transport layer is different from that of the first transport layer. Through this structure, the hole mobility is increased during the migration of hole carriers from the hole injection layer to the light-emitting layer. Mobility of hole carriers.

Benefits of technology

It effectively improves the stability of the light-emitting device, extends the service life of the display screen and electronic equipment, and improves the user experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118829263A_ABST
    Figure CN118829263A_ABST
Patent Text Reader

Abstract

The invention provides a light-emitting device, a display screen, electronic equipment and a preparation method of the light-emitting device, and relates to the technical field of screen display, the light-emitting device comprises a hole injection layer, a hole transport layer and a light-emitting layer which are stacked, and the hole transport layer is arranged along the direction from the hole injection layer to the light-emitting layer. The hole transport layer comprises a first transport layer, a second transport layer and a third transport layer which are stacked, the hole mobility of the third transport layer is greater than that of the second transport layer, and the hole mobility of the second transport layer is different from that of the first transport layer. According to the invention, the third transmission layer with the hole mobility greater than that of the second transmission layer is arranged, so that the mobility of the hole carriers is effectively improved in the process that the hole carriers migrate from the hole injection layer to the light-emitting layer, the stability of the light-emitting device is improved, and the use experience of a user is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of screen display technology, and in particular to a light-emitting device, a display screen, an electronic device, and a method for preparing the light-emitting device. Background Art

[0002] Currently, active-matrix organic light-emitting diodes (AMOLED) are widely used in various display devices due to their advantages such as ultra-thinness, flexibility, and low driving voltage. Among them, light-emitting devices are the key basic components for building various high-resolution, high-performance AMOLED display screens. However, as light-emitting devices work for a long time, the carrier migration efficiency will decrease, resulting in color deviation of the light-emitting devices, affecting the user experience. Summary of the invention

[0003] In order to overcome the problems existing in the related art, the present disclosure provides a light-emitting device, a display screen, an electronic device and a method for preparing the light-emitting device.

[0004] According to a first aspect of the present disclosure, a light-emitting device is provided, comprising a stacked hole injection layer, a hole transport layer and a light-emitting layer, wherein along a direction from the hole injection layer to the light-emitting layer, the hole transport layer comprises a stacked first transport layer, a second transport layer and a third transport layer, the hole mobility of the third transport layer is greater than the hole mobility of the second transport layer, and the hole mobility of the second transport layer is different from that of the first transport layer.

[0005] Optionally, the first transmission layer, the second transmission layer and the third transmission layer are all P-type organic semiconductor material layers, and the material constituting the third transmission layer is different from the material constituting the second transmission layer.

[0006] Optionally, the material of the third transmission layer and the material of the second transmission layer are both single materials.

[0007] Optionally, the light-emitting layer is configured to emit green light.

[0008] Optionally, a thickness ratio of the second transmission layer to the third transmission layer is 16:1 to 20:1.

[0009] Optionally, the thickness of the third transmission layer is 5 nm to 10 nm.

[0010] Optionally, the thickness of the first transmission layer is 125 nm to 140 nm; and / or,

[0011] The second transport layer has a thickness of 21 to 80 nm.

[0012] Optionally, the light emitting device is configured as a top emitting light emitting device.

[0013] Optionally, the light emitting device further includes a first light extraction layer and a second light extraction layer located on a light emitting side of the first light extraction layer along a light emitting direction, and the second light extraction layer is a lithium fluoride layer.

[0014] Optionally, the thickness of the first light extraction layer is 75nm to 80nm;

[0015] and / or,

[0016] The second light extraction layer has a thickness of 22 nm to 23 nm.

[0017] According to a second aspect of the present disclosure, a display screen is provided, wherein the display screen array is provided with the light-emitting device as described in the first aspect of the present disclosure.

[0018] According to a third aspect of the present disclosure, an electronic device is provided, wherein the electronic device comprises the display screen as described in the second aspect of the present disclosure.

[0019] According to a fourth aspect of the present disclosure, a method for preparing a light-emitting device is provided, for preparing the light-emitting device according to the first aspect of the present disclosure, the method for preparing the light-emitting device comprising:

[0020] forming an anode on the substrate;

[0021] forming a hole injection layer covering the anode;

[0022] forming a hole transport layer covering the hole injection layer, wherein the hole transport layer comprises a first transport layer, a second transport layer and a third transport layer which are stacked, the hole mobility of the third transport layer is greater than the hole mobility of the second transport layer, and the hole mobility of the second transport layer is different from that of the first transport layer;

[0023] forming a light-emitting layer covering the hole injection layer;

[0024] forming a hole blocking layer covering the light-emitting layer;

[0025] forming an electron transport layer covering the hole blocking layer;

[0026] forming an electron injection layer covering the electron transport layer;

[0027] A cathode is formed covering the electron injection layer.

[0028] Optionally, the forming of a hole transport layer covering the hole injection layer further comprises:

[0029] forming a first transport layer covering the anode;

[0030] forming a second transmission layer covering the first transmission layer;

[0031] A third transmission layer is formed covering the second transmission layer.

[0032] Optionally, the method for preparing the light-emitting device further includes:

[0033] forming a first light extraction layer covering the cathode;

[0034] A second light extraction layer is formed covering the first light extraction layer.

[0035] The technical solution provided by the embodiments of the present disclosure may include the following beneficial effects: the present disclosure sets a third transport layer with a hole mobility greater than that of the second transport layer to effectively improve the mobility of hole carriers during the migration of hole carriers from the hole injection layer to the light-emitting layer, which is beneficial to improving the stability of the light-emitting device and enhancing the user experience.

[0036] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0038] Figure 1 is a schematic structural diagram of a light emitting device according to an exemplary embodiment.

[0039] Figure 2 is a flow chart of a method for preparing a light emitting device according to an exemplary embodiment. DETAILED DESCRIPTION

[0040] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are merely examples of devices and methods consistent with some aspects of the present invention as detailed in the appended claims.

[0041] Currently, active-matrix organic light-emitting diodes (AMOLED) are widely used in various display devices due to their advantages such as ultra-thinness, flexibility, and low driving voltage. Among them, light-emitting devices are the key basic components for building various high-resolution, high-performance AMOLED display screens.

[0042] However, when the light-emitting device of the existing AMOLED display screen is powered on, the hole carrier transfer efficiency of the hole transport layer of the light-emitting device gradually decreases during the process of hole carrier migration from the anode to the light-emitting layer, thereby causing the hole carrier injection state in the light-emitting layer interface to deteriorate, and then color deviation occurs, which seriously affects the user experience.

[0043] In order to solve the above problems, the present disclosure provides a light-emitting device, a display screen, an electronic device and a method for preparing a light-emitting device, wherein the light-emitting device includes a stacked hole injection layer, a hole transport layer and a light-emitting layer, and along the direction from the hole injection layer to the light-emitting layer, the hole transport layer includes a stacked first transport layer, a second transport layer and a third transport layer, the hole mobility of the third transport layer is greater than the hole mobility of the second transport layer, and the hole mobility of the second transport layer is different from that of the first transport layer. The present disclosure effectively improves the mobility of hole carriers during the migration of hole carriers from the hole injection layer to the light-emitting layer by setting a third transport layer having a hole mobility greater than that of the second transport layer, which is beneficial to improving the stability of the light-emitting device and improving the user experience.

[0044] According to an exemplary embodiment, this embodiment provides a light-emitting device for use in an AMOLED display screen. The light-emitting device may be a top-emitting device, a bottom-emitting device, or a double-sided emitting device. Usually, except for the AMOLED display screen used in a television, other electronic devices using the AMOLED display screen all use top-emitting devices for arrangement and combination. This disclosure uses a top-emitting device as an example to illustrate the technical concept in this disclosure. The technical concept introduced below may also be applied to a bottom-emitting device or a double-sided emitting device.

[0045] like Figure 1 As shown, the light-emitting device in the present disclosure is a top-emitting device, and the light-emitting device includes a stacked hole injection layer 20, a hole transport layer 30 and a light-emitting layer 40. Figure 1 ), the hole transport layer 30 includes a first transport layer 31, a second transport layer 32 and a third transport layer 33 which are stacked, wherein the hole mobility of the third transport layer 33 is greater than the hole mobility of the second transport layer 32, and the hole mobility of the second transport layer 32 is different from that of the first transport layer 31.

[0046] Here, it should be noted that if only the first transmission layer 31 and the second transmission layer 32 are set, the migration performance of the holes will be reduced after the light-emitting device has been working for a long time, resulting in deviations in the color display. If the second transmission layer 32 is not set, and only the first transmission layer 31 and the third transmission layer 33 are set, the light-emitting device may display abnormally due to the excessively high efficiency of hole carrier migration. In order to change this situation, the present disclosure comprehensively considers setting the second transmission layer 32 and the third transmission layer 33, and the hole mobility of the third transmission layer 33 is higher than that of the second transmission layer 32. While ensuring that the hole carrier mobility is not too high or too low, the efficiency of the second transmission layer 32 in transporting hole carriers to the light-emitting layer 40 can also be improved, thereby improving the working reliability and stability of the display. In addition, since the thickness of the second transmission layer 32 and the third transmission layer 33 are related to the microcavity length of the light-emitting device and the carrier transmission rate, during the design stage of the light-emitting device, the thickness of the second transmission layer 32 and the third transmission layer 33 can be pre-set according to the relevant requirements of the light-emitting device, and then prepared according to the pre-set dimensions during the preparation process to ensure that the light-emitting effect of the light-emitting device is in the best state.

[0047] In some embodiments, the first transmission layer 31, the second transmission layer 32, and the third transmission layer 33 are all P-type organic semiconductor material layers, and the material constituting the third transmission layer 33 is different from the material constituting the second transmission layer 32. When selecting the material, it is necessary to ensure that the hole mobility of the material of the third transmission layer 33 is greater than the hole mobility of the material of the second transmission layer 32. In some embodiments, the material of the third transmission layer 33 and the material of the second transmission layer 32 are both single materials, wherein the single material refers to a material containing only one component, which is not doped with other materials, and the materials of the third transmission layer 33 and the second transmission layer 32 are different.

[0048] The material of the first transmission layer 31 and the second transmission layer 32 can be NPB (N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, chemical formula C 44 H 32 N2, CAS No. 123847-85-8), TPD (N,N'-diphenyl-N,N'-(3-methylphenyl)-1,1'-biphenyl-4,4'-diamine, chemical formula C 38 H 32 N2, CAS No. 65181-78-4), β-NPB (N,N'-di(naphthalene-2-yl)-N,N'-di(phenyl)biphenyl-4,4'-diamine, chemical formula C 44 H 32N2, CAS No. 139255-17-7) or other organic semiconductor materials. Preferably, the material constituting the first transport layer 31 is different from the material constituting the second transport layer 32. The hole mobility of the second transport layer 32 may be greater than the hole mobility of the first transport layer 31, or may be less than the hole mobility of the first transport layer 31. Even in some special cases, the material of the first transport layer 31 and the material of the second transport layer 32 may be different, but the hole mobility of the two may be substantially the same, and the present disclosure does not impose any special restrictions on this.

[0049] In one example, the hole mobility of the third transport layer 33 is higher than that of the second transport layer 32, and the third transport layer may be formed of TTP (chemical formula C 10 H 17 N2O 15 P3, CAS No. 80223-29-6), TAPC (4,4'-cyclohexylbis[N,N-di(4-methylphenyl)aniline], chemical formula C 46 H 46 N2, CAS No. 1174006-36-0) or other materials. It should be noted that when selecting the materials of the second transmission layer 32 and the third transmission layer 33, it is necessary to ensure that the hole mobility of the material constituting the third transmission layer 33 is higher than the hole mobility of the material constituting the second transmission layer 32.

[0050] In some embodiments, the thickness of the second transmission layer 32 and the third transmission layer 33 are related to the transmission rate of the light-emitting device and the microcavity length of the light-emitting device, wherein the microcavity length of the light-emitting device refers to the total thickness of all film layers between the anode and the cathode of the light-emitting device, and the microcavity length directly affects the light-emitting effect of the light-emitting device. Therefore, when designing the light-emitting device, the thickness of the second transmission layer 32 and the third transmission layer 33 can be pre-designed, which is more conducive to adjusting the microcavity length to the optimal optical path.

[0051] In some embodiments, the first transmission layer 31, the second transmission layer 32, and the third transmission layer 33 may have different thicknesses. Once the thicknesses of the first transmission layer 31, the second transmission layer 32, and the third transmission layer 33 are set in the design stage of the light-emitting device, they will no longer change. However, since the thicknesses of the second transmission layer 32 and the third transmission layer 33 will affect the carrier transmission efficiency of the light-emitting device during subsequent use, in order to obtain better technical effects, the second transmission layer 32 and the third transmission layer 33 may be set according to the following ratio, so as to obtain the purpose of better improving the light-emitting effect of the light-emitting device. The thickness ratio between the second transmission layer 32 and the third transmission layer 33 is 16:1 to 20:1. When setting the second transmission layer 32 and the third transmission layer 33, the thickness of one of the layers may be set first, and then the thickness of the other layer may be set according to the above ratio.

[0052] Exemplarily, the thickness of the third transmission layer 33 is 5nm to 10nm, preferably 5nm to 8nm; the thickness of the first transmission layer 31 is 125nm to 140nm; and / or the thickness of the second transmission layer 32 is 21 to 80nm, preferably 21 to 21.6nm.

[0053] In one example, the thickness is 80 nm, the second transmission layer 32 and the third transmission layer 33 are arranged in a ratio of 16:1, and the thickness of the third transmission layer is 5 nm.

[0054] In one example, the thickness of the third transmission layer 33 may include but is not limited to 5.0 nm, 5.5 nm, 6.0 nm, 6.5 nm, 7.0 nm, 7.5 nm, 8.0 nm, the thickness of the second transmission layer 32 may include but is not limited to 21.0 nm, 21.3 nm, 21.6 nm, and the thickness of the first transmission layer 31 may include but is not limited to 133.7 nm, 134.0 nm, 134.3 nm. In one example, the thickness of the third transmission layer 33 is 6 nm, the thickness of the first transmission layer 31 is 134 nm, and the thickness of the second transmission layer 32 is 21.5 nm. In another example, the thickness of the third transmission layer 33 is 5 nm to 8 nm, and the thickness of the first transmission layer 31 is 134 ± 0.3 nm. For example, the thickness of the third transmission layer 33 is 5 nm, the thickness of the first transmission layer 31 is 133.8 nm, and the thickness of the second transmission layer 32 is not limited, and can be selected by those skilled in the art as needed. In another example, the thickness of the third transmission layer 33 is 5 nm to 8 nm, and the thickness of the second transmission layer 32 is 21 to 21.6 nm. For example, the thickness of the third transmission layer 33 is 8 nm, and the thickness of the second transmission layer 32 is 21.3 nm. The thickness of the first transmission layer 31 is not limited and can be selected by those skilled in the art as needed. Of course, it can be understood that the thickness of the first transmission layer 31, the second transmission layer 32 and the third transmission layer 33 is not limited to the values, proportions and ranges listed in this embodiment, and those skilled in the art can adjust the thickness of the first transmission layer 31, the second transmission layer 32 and the third transmission layer 33 as needed.

[0055] In some embodiments, the hole injection layer 20 is disposed on the upstream side of the first transmission layer 31 along the light emission direction. Figure 1 As shown, the hole injection layer 20 is disposed below the first transport layer 31. The hole injection layer 20 is used to reduce the barrier for hole injection from the anode so that the holes can be effectively injected from the anode into the light-emitting layer. The thickness of the hole injection layer 20 is 5nm to 10nm, including but not limited to 5nm, 6nm, 7nm, 8nm, 9nm, 10nm. The hole injection layer 20 is configured to be a doped P-type semiconductor organic material, wherein the main material of the hole injection layer 20 is an organic small molecule semiconductor material, such as NPB, TPD, β-NPB or other organic semiconductor materials; the guest material of the hole injection layer 20 can be F4-TCNQ (2,3,5,6-tetrafluoro-7,7',8,8'-tetracyanoquinone-dimethane, chemical formula C 12 F4N4, CAS No. 29261-33-4), HAT-CN (chemical formula C 18 N 12, CAS No. 105598-27-4) and other materials. Among them, the doping concentration mass ratio of the guest material is 0.5% to 1.5%, including but not limited to 0.5%, 0.75%, 1.0%, and 1.5%. Of course, it can be understood that the host material and the guest material of the hole injection layer 20 are not limited to the materials listed in the present disclosure, and those skilled in the art can choose according to actual needs.

[0056] In some embodiments, reference Figure 1 As shown, the light emitting device is configured as a top emitting light emitting device, the light emitter 10 is an anode, the light receiving electrode 80 is a cathode, and the light emitter 10 is arranged on the upstream side of the hole injection layer 20 along the light emission direction. Figure 1 The light emitter 10 is arranged below the hole injection layer 20 to emit holes to the light emitting layer 40, wherein the light emitter 10 is composed of a first deposition layer 11, a second deposition layer 12 and a third deposition layer 13, along the direction in which the light is emitted, that is, Figure 1 As shown in the figure, from bottom to top, the first deposition layer 11, the second deposition layer 12 and the third deposition layer 13 are stacked in sequence. Exemplarily, the material of the first deposition layer 11 and the third deposition layer 13 is indium tin oxide, and the material of the second deposition layer 12 is silver, wherein the thickness of the first deposition layer 11 is 7nm to 10nm, the thickness of the second deposition layer 12 is 100nm to 120nm, and the thickness of the third deposition layer 13 is 8nm to 12nm, and the thin film process technology of the first deposition layer 11, the second deposition layer 12 and the third deposition layer 13 all adopts magnetron sputtering. It can be understood that the material, thickness and process of the first deposition layer 11, the second deposition layer 12 and the third deposition layer 13 can be selected by those skilled in the art according to actual needs, and the present disclosure does not impose any special restrictions on this.

[0057] In some embodiments, the light emitting layer 40 is used to emit light, and along the light emission direction, the hole transport layer 30 is located on the upstream side of the light emitting layer 40. Figure 1 Based on the orientation shown, the hole transport layer 30 is arranged below the light-emitting layer 40, and the light-emitting layer 40 is arranged as a doped light-emitting material. For example, the main material of the doped light-emitting material is an organic small molecule light-emitting material, and the guest material is a phosphorescent material, a heavy metal material, such as iridium, platinum and other materials. The mass ratio of the guest material is 6% to 10%, including but not limited to 6%, 7%, 8%, 9%, 10%; the thickness of the light-emitting layer 40 is 35nm to 42nm, including but not limited to 37nm, 38nm, 39nm, 40nm, 42nm. In addition, the light-emitting layer 40 is also arranged to emit green light. Of course, it can be understood that the light-emitting layer 40 can also be arranged to emit blue light, red light, etc., and the present disclosure does not impose too many restrictions on this.

[0058] In some embodiments, the light emitting device further includes a hole blocking layer 50. The hole blocking layer 50 is used to block the carriers from continuing to migrate after passing through the light emitting layer 40, so as to prevent the hole carrier concentration in the light emitting layer 40 from decreasing, thereby reducing the light emitting efficiency and affecting the normal operation of the light emitting device. In the direction in which the light is emitted, the hole blocking layer 50 is disposed on the downstream side of the light emitting layer 40 to prevent the hole blocking layer 50 from continuing to migrate after passing through the light emitting layer 40. Figure 1 The hole blocking layer 50 is disposed above the light emitting layer 40. The hole blocking layer 50 is an organic semiconductor material, such as BCP (2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline, chemical formula C 26 H 20 N2, CAS No. 4733-39-5), BAlq (bis(2-methyl-8-hydroxyquinoline-N1,O8)-(1,1'-biphenyl-4-hydroxy)aluminum, chemical formula C 32 H 25 AlN2O3, CAS No. 146162-54-1) or other materials, the thickness of the hole blocking layer 50 can be 5nm to 10nm, including but not limited to 5nm, 7nm, 10nm.

[0059] In some embodiments, the light emitting device further includes an electron transport layer 60. The electron transport layer 60 is used to increase the migration rate of electrons so that the electrons injected from the cathode and the holes injected from the anode can be recombined in the light emitting layer. In the direction in which the light is emitted, the electron transport layer 60 is disposed on the downstream side of the hole blocking layer 50 to Figure 1 The electron transport layer 60 is disposed above the hole blocking layer 50. The electron transport layer 60 is a doped electron transport material. The host material of the doped electron transport material may be Liq (8-hydroxyquinoline-lithium, chemical formula C9H6LiNO, CAS number 850918-68-2), and the guest material may be TPBi (1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl)benzene, chemical formula C 45 H 30 N6, CAS No. 192198-85-9), Bphen (4,7-diphenyl-1,10-phenanthroline, chemical formula C 24 H 16 N2, CAS No. 1662-01-7) and other materials. Among them, the mass proportion of Liq is 40% to 50%, including but not limited to 40%, 45%, and 50%. The thickness of the electron transport layer 60 is 30nm to 40nm, including but not limited to 30nm, 35nm, and 40nm.

[0060] In some embodiments, the light emitting device further includes an electron injection layer 70. In the direction in which the light is emitted, the electron injection layer 70 is disposed on the downstream side of the electron transport layer 60 so as to Figure 1Based on the orientation shown, the electron injection layer 70 is disposed above the electron transport layer 60. The electron injection layer 70 is used to reduce the barrier for injecting electrons from the cathode so that the electrons can be effectively injected from the cathode into the light-emitting device. Exemplarily, the material of the electron injection layer 70 is metal ytterbium (Yb), and the thickness of the electron injection layer 70 is 0.8nm to 1.0nm, including but not limited to 0.8nm, 0.9nm, and 1.0nm.

[0061] In some embodiments, the light emitting device further includes a light receiving electrode 80. Taking a top-emitting light emitting device as an example, the light receiving electrode 80 is a metal cathode. Along the direction in which the light is emitted, the light receiving electrode 80 is disposed on the downstream side of the electron injection layer 70 to Figure 1 Based on the orientation shown, the light receiving electrode 80 is arranged above the electron injection layer 70, and the light receiving electrode 80 is made of metal. Exemplarily, the light receiving electrode 80 is formed of a mixed material of magnesium (Mg) and silver (Ag), wherein the mass ratio of magnesium to silver is 1:9, and the thickness of the light receiving electrode 80 is 12.1nm to 13.2nm, including but not limited to 12.1nm, 12.3nm, 12.5nm, 12.7nm, 13.0nm, 13.2nm. The specific material and thickness of the light receiving electrode 80 can be selected by those skilled in the art according to actual needs, and the present disclosure does not impose too many restrictions on this.

[0062] In some embodiments, the light extraction layer 90 of the light emitting device includes a first light extraction layer 91 and a second light extraction layer 92. In the light emission direction, the first light extraction layer 91 is disposed on the downstream side of the light receiving electrode 80, and the second light extraction layer 92 is located on the light emitting side of the first light extraction layer 91. The second light extraction layer 92 is a lithium fluoride layer. Figure 1 Based on the orientation shown, the first light extraction layer 91 is arranged above the light receiving electrode 80, and the second light extraction layer 92 is arranged above the first light extraction layer 91. Among them, the material of the first light extraction layer 91 is an organic semiconductor material, and the material of the first light extraction layer 91 can use any one of the materials used to prepare the first transmission layer 31, the second transmission layer 32 and the third transmission layer 33. The thickness of the first light extraction layer 91 is 75nm to 80nm; and / or, the thickness of the second light extraction layer 92 is 22nm to 23nm. In this embodiment, the second light extraction layer 92 is provided to increase the light refractive index and improve the light emitting effect of the light emitting device. Above the second light extraction layer 92 (with Figure 1 The encapsulation layer can also be set.

[0063] In one example, the material of the first light extraction layer 91 is NPB, and the thickness of the first light extraction layer 91 is 75nm to 80nm, including but not limited to 75nm, 76nm, 77nm, 78nm, 79nm, and 80nm; the thickness of the second light extraction layer 92 is 22nm to 23nm, including but not limited to 22nm, 22.5nm, and 23nm. In another example, the material of the first light extraction layer 91 is BCP, and the thickness of the second light extraction layer 92 is 22nm to 23nm. In yet another example, the material of the first light extraction layer 91 is TPBi, and the thickness of the first light extraction layer 91 is 75nm to 80nm, and the thickness of the second light extraction layer 92 is 22.5nm. Of course, it can be understood that the specific material and thickness of the first light extraction layer 91 and the second light extraction layer 92 can be selected by those skilled in the art according to actual needs, and the present disclosure does not impose too many restrictions on this.

[0064] In one example, the hole injection layer 20, the first transport layer 31, the second transport layer 32, the third transport layer 33, the light-emitting layer 40, the hole blocking layer 50, the electron transport layer 60, the electron injection layer 70, the light receiving electrode 80, the first light extraction layer 91 and the second light extraction layer 92 are all prepared by vacuum thermal evaporation.

[0065] refer to Figure 1 As shown, the working principle of the embodiment of the present disclosure is explained below by taking a top-emitting device as an example.

[0066] Along the direction of the light, that is Figure 1 As shown in the figure, from bottom to top, a light emitter 10, a hole injection layer 20, a hole transport layer 30, a light emitting layer 40, a hole blocking layer 50, an electron transport layer 60, an electron injection layer 70, a light receiving electrode 80 and a light extraction layer 90 are sequentially arranged. The light emitter 10 is an anode, the light receiving electrode 80 is a cathode, and the electrons injected by the cathode are directed along the Figure 1 The holes injected by the anode are transported from top to bottom to the light-emitting layer 40. Figure 1 The electrons and holes are recombined in the light-emitting layer 40, so that the material of the light-emitting layer 40 generates light, and the light-emitting device emits light.

[0067] The light emitter 10 is used to emit holes to the light emitting layer 40, the hole injection layer 20 is used to reduce the potential barrier of the anode injecting holes so that the holes can be effectively injected from the anode into the light emitting layer, the hole transport layer 30 is used to transport holes, and the hole blocking layer 50 is used to block the holes from continuing to migrate after passing through the light emitting layer 40, so as to avoid the hole carrier concentration in the light emitting layer 40 from decreasing, resulting in a decrease in the luminous efficiency, and affecting the normal operation of the light emitting device. The light receiving electrode 80 is used to generate electrons, the electron injection layer 70 is used to reduce the potential barrier of injecting electrons from the cathode so that the electrons can be effectively injected from the cathode into the light emitting device, and the electron transport layer 60 is used to increase the migration rate of the electrons. Among them, the hole transport layer 30 includes a first transport layer 31, a second transport layer 32 and a third transport layer 33 arranged in sequence from bottom to top, and the setting of the thickness of the second transport layer 32 and the third transport layer 33 will affect the hole transmission rate of the light emitting device and the microcavity length of the light emitting device, but once the thickness of the second transport layer 32 and the third transport layer 33 is set, it will not change. The light extraction layer 90 includes a first light extraction layer 91 and a second light extraction layer 92 which are sequentially arranged from bottom to top. The second light extraction layer 92 is used to increase the light refractive index and improve the light extraction effect of the light emitting device.

[0068] The technical concept introduced in the present disclosure can also be applied to bottom-emitting devices or double-sided emitting devices. The light-emitting devices in the present disclosure can be used alone or in combination in an array to display different contents on a display screen using the array combination.

[0069] According to an exemplary embodiment, still referring to Figure 1 This embodiment provides a display screen (not shown in the figure), and the display screen array is provided with the light-emitting device described in the above embodiment. The light-emitting device is suitable for FHD (Full High Definition, FHD, full high definition) resolution AMOLED display screens, and is also suitable for FHD+ and QHD (Quarter High Definition, QHD, 1 / 4 of the full high definition resolution) resolution AMOLED display screens, and the pixel gap range used by the light-emitting device is 15.0μm to 22.0μm.

[0070] According to another exemplary embodiment, still referring to Figure 1 This embodiment provides an electronic device (not shown in the figure), which includes the display screen described in the above embodiment.

[0071] According to an exemplary embodiment, Figure 2 As shown, this embodiment provides a method for preparing a light-emitting device, and the method for preparing a light-emitting device includes:

[0072] S10, forming an anode on the substrate.

[0073] Wherein, the anode is composed of a first deposition layer, a second deposition layer and a third deposition layer, and the first deposition layer, the second deposition layer and the third deposition layer are sequentially formed on the substrate. Exemplarily, the material of the first deposition layer and the third deposition layer is indium tin oxide, the material of the second deposition layer is silver, the thickness of the first deposition layer is 7nm to 10nm, the thickness of the second deposition layer is 100nm to 120nm, and the thickness of the third deposition layer is 8nm to 12nm. The thin film process technology of the first deposition layer, the second deposition layer and the third deposition layer all adopts magnetron sputtering. It can be understood that the material, thickness and process of the first deposition layer, the second deposition layer and the third deposition layer can be selected by those skilled in the art according to actual needs, and the present disclosure does not impose any special restrictions on this.

[0074] S20, forming a hole injection layer covering the anode.

[0075] The hole injection layer is prepared by vacuum thermal evaporation, the hole injection layer is set to be doped with P-type semiconductor organic material, the main material of the hole injection layer is an organic small molecule semiconductor material, such as NPB, TPD, β-NPB or other organic semiconductor materials; the guest material of the hole injection layer can be F4-TCNQ, HAT-CN and other materials, and the doping concentration mass ratio of the guest material is 0.5% to 1.5%, including but not limited to 0.5%, 0.75%, 1.0%, 1.5%. The thickness of the hole injection layer is 5nm to 10nm, including but not limited to 5nm, 6nm, 7nm, 8nm, 9nm, 10nm.

[0076] S30, forming a hole transport layer covering the hole injection layer, wherein the hole transport layer includes a first transport layer, a second transport layer and a third transport layer which are stacked, the hole mobility of the third transport layer is greater than the hole mobility of the second transport layer, and the hole mobility of the second transport layer is different from that of the first transport layer.

[0077] Wherein, the material of the third transmission layer and the material of the second transmission layer are both single materials. Preferably, the materials of the third transmission layer and the second transmission layer are both single materials, and the materials of the third transmission layer and the second transmission layer are different. The first transmission layer, the second transmission layer and the third transmission layer are all P-type organic semiconductor material layers, formed by vacuum thermal evaporation. It should be noted that when selecting the materials of the second transmission layer and the third transmission layer, it is necessary to ensure that the hole mobility of the material constituting the third transmission layer is higher than the hole mobility of the material constituting the second transmission layer.

[0078] S40, forming a light-emitting layer covering the hole injection layer.

[0079] Among them, the light-emitting layer is a doped light-emitting material, which is prepared by vacuum thermal evaporation. Exemplarily, the main material of the doped light-emitting material is an organic small molecule light-emitting material, and the guest material is a phosphorescent material, a heavy metal material, such as iridium, platinum and other materials. The mass ratio of the guest material is 6% to 10%, including but not limited to 6%, 7%, 8%, 9%, 10%; the thickness of the light-emitting layer is 35nm to 42nm, including but not limited to 37nm, 38nm, 39nm, 40nm, 42nm. In addition, the light-emitting layer is configured to emit green light. Of course, it can be understood that the light-emitting layer can also be configured to emit blue light, red light, etc., and the present disclosure does not impose too many restrictions on this.

[0080] S50, forming a hole blocking layer covering the light-emitting layer.

[0081] The hole blocking layer is an organic semiconductor material prepared by vacuum thermal evaporation. The hole blocking layer can be made of, for example, BCP, BAlq or other materials, and the thickness of the hole blocking layer can be 5nm to 10nm, including but not limited to 5nm, 7nm, and 10nm.

[0082] S60, forming an electron transport layer covering the hole blocking layer.

[0083] The electron transport layer is prepared by vacuum thermal evaporation. The electron transport layer is a doped electron transport material. The main material of the doped electron transport material can be Liq, and the guest material can be TPBi, Bphen and other materials. The mass proportion of Liq is 40% to 50%, including but not limited to 40%, 45%, and 50%. The thickness of the electron transport layer is 30nm to 40nm, including but not limited to 30nm, 35nm, and 40nm.

[0084] S70, forming an electron injection layer covering the electron transport layer.

[0085] The electron injection layer is prepared by vacuum thermal evaporation. Exemplarily, the material of the electron injection layer is metal ytterbium (Yb), and the thickness of the electron injection layer is 0.8 nm to 1.0 nm, including but not limited to 0.8 nm, 0.9 nm, and 1.0 nm.

[0086] S80, forming a cathode covering the electron injection layer.

[0087] The cathode is prepared by vacuum thermal evaporation. Exemplarily, the cathode is formed of a mixed material of magnesium (Mg) and silver (Ag), wherein the mass ratio of magnesium to silver is 1:9, and the thickness of the light receiving electrode is 12.1nm to 13.2nm, including but not limited to 12.1nm, 12.3nm, 12.5nm, 12.7nm, 13.0nm, 13.2nm,

[0088] In some embodiments, step S30, forming a hole transport layer covering the hole injection layer further comprises:

[0089] S301, forming a first transport layer covering the anode.

[0090] Among them, the first transmission layer is a P-type organic semiconductor material layer, which is formed by vacuum thermal evaporation. The material of the first transmission layer can be NPB, TPD, β-NPB or other organic semiconductor materials, and the thickness is 134±0.3nm.

[0091] S302, forming a second transmission layer covering the first transmission layer.

[0092] Among them, the second transmission layer is a P-type organic semiconductor material layer, which is formed by vacuum thermal evaporation. The material of the second transmission layer can be NPB, TPD, β-NPB or other organic semiconductor materials, and the thickness of the second transmission layer 32 is 21 to 21.6 nm. Preferably, the material constituting the second transmission layer is different from the material constituting the first transmission layer, and the hole mobility of the second transmission layer can be greater than the hole mobility of the first transmission layer, or less than the hole mobility of the first transmission layer. Even in some special cases, the material of the first transmission layer and the material of the second transmission layer can be different, but the hole mobility of the two can be roughly the same, and the present disclosure does not impose any special restrictions on this.

[0093] S303, forming a third transmission layer covering the second transmission layer.

[0094] Among them, the third transmission layer is a P-type organic semiconductor material layer, which is formed by vacuum thermal evaporation. The material of the third transmission layer can be TTP, TAPC or other materials. The thickness of the third transmission layer 33 is 5nm to 8nm. The material of the third transmission layer is different from the material of the second transmission layer. The material of the third transmission layer can be the same as or different from the material of the first transmission layer. When selecting the material, it is necessary to ensure that the hole mobility of the material of the third transmission layer is greater than the hole mobility of the material of the second transmission layer.

[0095] In some embodiments, the method for preparing a light emitting device further includes:

[0096] A first light extraction layer is formed covering the cathode.

[0097] A second light extraction layer is formed covering the first light extraction layer.

[0098] Among them, the first light extraction layer is formed by vacuum thermal evaporation. The material of the first light extraction layer can be selected from any organic semiconductor material used in the above layers. The thickness of the first light extraction layer is 75nm to 80nm, including but not limited to 75nm, 76nm, 77nm, 78nm, 79nm, and 80nm.

[0099] The second light extraction layer is formed by vacuum thermal evaporation, and the material of the second light extraction layer can be selected from any organic semiconductor material used in the above layers, and the thickness of the second light extraction layer is 22nm to 23nm, including but not limited to 22nm, 22.5nm, and 23nm. The first light extraction layer and the second light extraction layer are used together to improve the light extraction effect.

[0100] Of course, it is understandable that during the preparation of the light-emitting device, the specific material, thickness and process of each layer can be selected by those skilled in the art according to actual needs, and the present disclosure does not impose too many restrictions on this.

[0101] In addition, a packaging layer may be further arranged on the second light extraction layer to form a complete light-emitting device. The process for forming the packaging layer may be consistent with the related technology and will not be described in detail.

[0102] The present disclosure provides a light-emitting device, a display screen, an electronic device, and a method for preparing the light-emitting device. The light-emitting device includes a stacked hole injection layer, a hole transport layer, and a light-emitting layer. In the direction from the hole injection layer to the light-emitting layer, the hole transport layer includes a first transport layer, a second transport layer, and a third transport layer stacked along the light emission direction. The hole mobility of the third transport layer is greater than the hole mobility of the second transport layer, and the hole mobility of the second transport layer is different from that of the first transport layer. The present disclosure effectively improves the mobility of hole carriers during the migration of hole carriers from the hole injection layer to the light-emitting layer by setting a third transport layer having a hole mobility greater than that of the second transport layer, which is beneficial to improving the stability of the light-emitting device, extending the service life of the display screen and the electronic device, and improving the user experience.

[0103] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the embodiments disclosed herein. This application is intended to cover any variations, uses, or adaptations of the present disclosure that follow the general principles of the present disclosure and include common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The specification and examples are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the following claims.

[0104] It should be understood that the present invention is not limited to the exact construction that has been described above and shown in the drawings and that various modifications and changes may be made without departing from the scope thereof. The scope of the present invention is limited only by the appended claims.

Claims

1. A light emitting device, characterized in that: The light-emitting device includes a stacked hole injection layer, a hole transport layer and a light-emitting layer. Along the direction from the hole injection layer to the light-emitting layer, the hole transport layer includes a stacked first transport layer, a second transport layer and a third transport layer. The hole mobility of the third transport layer is greater than the hole mobility of the second transport layer, and the hole mobility of the second transport layer is different from that of the first transport layer.

2. The light emitting device according to claim 1, characterized in that: The first transmission layer, the second transmission layer and the third transmission layer are all P-type organic semiconductor material layers, and the material constituting the third transmission layer is different from the material constituting the second transmission layer.

3. The light emitting device according to claim 1, characterized in that: The material of the third transmission layer and the material of the second transmission layer are both single materials.

4. The light emitting device according to any one of claims 1 to 3, characterized in that: The light emitting layer is configured to emit green light.

5. The light emitting device according to any one of claims 1 to 3, characterized in that: The thickness ratio of the second transmission layer to the third transmission layer is 16:1 to 20:

1.

6. The light emitting device according to any one of claims 1 to 3, characterized in that: The thickness of the third transmission layer is 5 nm to 10 nm.

7. The light emitting device according to any one of claims 1 to 3, characterized in that: The thickness of the first transmission layer is 125 nm to 140 nm; and / or, The second transport layer has a thickness of 21 to 80 nm.

8. The light emitting device according to any one of claims 1 to 3, characterized in that: The light emitting device is configured as a top emitting light emitting device.

9. The light emitting device according to claim 8, characterized in that: The light emitting device further includes a first light extraction layer and a second light extraction layer located on a light emitting side of the first light extraction layer along a light emitting direction, wherein the second light extraction layer is a lithium fluoride layer.

10. The light emitting device according to claim 9, characterized in that: The thickness of the first light extraction layer is 75nm to 80nm; and / or, The second light extraction layer has a thickness of 22 nm to 23 nm.

11. A display screen, characterized in that: The display screen array is provided with the light emitting device according to any one of claims 1 to 10.

12. An electronic device, characterized in that: The electronic device comprises the display screen as claimed in claim 11.

13. A method for preparing a light emitting device, characterized in that: Used to prepare the light-emitting device according to any one of claims 1 to 10, the preparation method of the light-emitting device comprising: forming an anode on the substrate; forming a hole injection layer covering the anode; forming a hole transport layer covering the hole injection layer, wherein the hole transport layer comprises a first transport layer, a second transport layer and a third transport layer which are stacked, the hole mobility of the third transport layer is greater than the hole mobility of the second transport layer, and the hole mobility of the second transport layer is different from that of the first transport layer; forming a light-emitting layer covering the hole injection layer; forming a hole blocking layer covering the light-emitting layer; forming an electron transport layer covering the hole blocking layer; forming an electron injection layer covering the electron transport layer; A cathode is formed covering the electron injection layer.

14. The method for preparing a light emitting device according to claim 13, characterized in that: The forming of a hole transport layer covering the hole injection layer further comprises: forming a first transport layer covering the anode; forming a second transmission layer covering the first transmission layer; A third transmission layer is formed covering the second transmission layer.

15. The method for preparing a light emitting device according to claim 13, characterized in that: The method for preparing the light emitting device further comprises: forming a first light extraction layer covering the cathode; A second light extraction layer is formed covering the first light extraction layer.