Method capable of prolonging service life of 7-series aluminum alloy mold

Through normalizing, tempering and nitriding treatment of forged steel materials, combined with the design of shunt holes and reinforcing structures, the problem of 7 series aluminum alloy mold fracture is solved, significantly extending the mold life and reducing production costs.

CN118831989APending Publication Date: 2024-10-25GUANGDONG JMA ALUMINUM PROFILE FACTORY GRP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410835739.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

7 series aluminum alloy molds are prone to breakage during use, resulting in short service life and high production costs. It is difficult to effectively solve this problem with existing technology.

Method used

Forged steel is used as the mold material, normalized and tempered to improve hardness and toughness, and a nitrided layer with a depth of 220-310μm is formed through nitriding treatment to prevent the diffusion of Zn ions in the 7 series aluminum alloy, combined with shunt holes and strengthen structural design to optimize mold structure and process.

Benefits of technology

It significantly extends the service life of the mold, reduces production costs, improves market competitiveness, and increases the mold life by more than 30 times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118831989A_ABST
    Figure CN118831989A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of aluminum alloy extrusion, and discloses a method capable of prolonging the service life of a 7-series aluminum alloy die, the die is a divergent die, and the method comprises the steps that forging steel is selected as a raw material to be machined, and the die is obtained; the mold is subjected to normalizing treatment and tempering treatment, the hardness of the mold reaches 44-48 HRC, the temperature of normalizing treatment ranges from 850 DEG C to 870 DEG C, and the temperature of tempering treatment ranges from 600 DEG C to 620 DEG C; and carrying out nitriding treatment on the mold, wherein the depth of a nitriding layer obtained by nitriding treatment is 220-310 [mu] m. By implementing the treatment method, the hardness of the mold and the residual stress in the mold can be reduced, the toughness of the mold is improved, the service life of the mold is obviously prolonged, the mold cost can be greatly saved, the product production cost is reduced, and the market competitiveness is improved. In addition, the mold treatment method is simple, high in operability, effective and capable of being used and popularized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy extrusion, and in particular to a method for improving the service life of a 7 series aluminum alloy mold. Background Art

[0002] Deformed aluminum alloys have high specific strength, high toughness, good processing performance and excellent corrosion resistance, and are widely used in aerospace, rail transit, automobiles, and civil construction. As a hard alloy, 7-series aluminum alloys are used in load-bearing or pressure-bearing structural products with relatively high material performance requirements. In terms of lightweight weight reduction, not only material weight reduction is sought, but also the structure is optimized and designed to reduce weight. Therefore, many 7-series aluminum alloy products also have cavity structures. The molds for producing cavity structure products are called diverter molds. Due to the high degree of alloying and poor metal fluidity of 7-series aluminum alloys, when extruding products with cavity structures, the molds are subjected to huge three-dimensional compressive stress, and the mold bridge has a great tendency to break, which puts higher requirements on the performance of the mold. Usually, the output of extruded products of 7-series alloys is 300-500kg / set of molds, which leads to very high mold costs, so the economic benefits are also relatively poor. However, 7-series aluminum alloy cavity products have huge market prospects. Breaking through the mold life limit, increasing its output, and reducing production costs are technical problems that aluminum processing companies are currently urgently trying to solve.

[0003] In the past, manufacturers could only seek better mold materials, such as forged steel, to manufacture molds, but the effect was not obvious. Usually, mold cracks occurred after 1 to 3 times of use. Therefore, the only way to make up for the disadvantage of insufficient mold life was to increase the number of molds, but this undoubtedly brought high production costs to the company. There are also ways to thicken the mold bridge to improve mold strength, to expand the mold diversion hole to reduce extrusion pressure, to shorten the working belt to reduce friction, to nitride the mold to improve mold fatigue strength, and to improve metal fluidity by improving the extrusion process. However, no matter whether it is a single method or a comprehensive method, it is not enough to fundamentally solve the problem of short mold life, and the problem of mold cracks is still frequent. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for improving the service life of 7 series aluminum alloy molds, so that the service life of 7 series aluminum alloy molds is significantly increased, the production cost of 7 series aluminum alloys is saved, and the method is highly operable.

[0005] In order to solve the above technical problems, the present invention provides a method for improving the service life of a 7 series aluminum alloy mold, wherein the mold is a split die mold, comprising:

[0006] Select forged steel as raw material for processing to obtain a mold;

[0007] The mold is subjected to normalizing and tempering treatments to make the hardness of the mold reach 44-48HRC, wherein the temperature of the normalizing treatment is 850-870°C, and the temperature of the tempering treatment is 600-620°C;

[0008] The mold is subjected to nitriding treatment, and the depth of the nitrided layer obtained by the nitriding treatment is 220 to 310 μm.

[0009] As an improvement of the above scheme, the specific steps of the nitriding treatment include:

[0010] (1) nitriding the newly produced mold;

[0011] (2) A short bar of 7 series aluminum alloy was extruded for one cycle using a nitrided die;

[0012] (3) removing the nitrided layer formed by the nitriding treatment and re-performing the nitriding treatment;

[0013] (4) Repeat steps (2) and (3).

[0014] As an improvement of the above solution, the forging steel includes 45A steel, 35CrMoL steel, stainless steel, and 4Cr3Mo3SiV steel.

[0015] As an improvement of the above scheme, the forging steel is selected as the raw material for processing to obtain the mold, which includes:

[0016] Select forged steel as raw material for processing to obtain the mold body;

[0017] A diverter hole with a flared shape is arranged on the mold body, and the diameter of the diverter hole gradually decreases from the inlet end to the outlet end.

[0018] As an improvement of the above solution, the step of selecting forged steel as raw material for processing to obtain a mold further comprises:

[0019] A shunt bridge and a welding chamber are arranged in the mold body. A reinforcement structure is arranged at a bridge position of the shunt bridge close to one end of the welding chamber, and the reinforcement structure includes a stainless steel layer.

[0020] As an improvement of the above scheme, the holding time of the normalizing treatment is 12 to 24 hours, and the cooling rate is 35 to 45°C / h.

[0021] The tempering treatment time is 0.5 to 2 hours, the cooling rate is 2 to 4° C. / s, and the tempering treatment times are 2 to 5 times.

[0022] As an improvement of the above solution, the depth of the nitrided layer obtained by the nitridation treatment is 220 to 240 μm.

[0023] As an improvement of the above scheme, the nitriding treatment is carried out twice. The first nitriding treatment makes the depth of the nitriding layer reach 130-150 μm, and the second nitriding treatment is continued so that the depth of the nitriding layer after the nitriding treatment reaches 220-240 μm.

[0024] As an improvement of the above solution, the gas introduced into the nitriding treatment is ammonia, and the temperature of the nitriding treatment is 500-560°C.

[0025] As an improvement of the above solution, one cycle is to extrude 140 to 160 7 series aluminum alloy short bars using the die.

[0026] The implementation of the present invention has the following beneficial effects:

[0027] In the present invention, forging steel is selected as raw material for processing to obtain a mold, so that the mold itself has a higher hardness and can withstand greater pressure; and the mold is normalized and tempered to make the hardness of the mold reach 44-48HRC, wherein the temperature of the normalizing treatment is 850-870°C, and the temperature of the tempering treatment is 600-620°C, which can reduce the hardness of the mold and the residual stress inside the mold, and improve the toughness of the mold. By nitriding the mold, the depth of the nitrided layer obtained by the nitriding treatment is 220-310μm, which can fully prevent the high-content Zn ions in the 7 series aluminum alloy from being able to the mold matrix, avoid cracking and catalysis of the mold during use, and significantly increase the life of the mold, which can greatly save the mold cost, reduce the product production cost, and improve the market competitiveness. In addition, the processing method of the mold in the present invention is simple, highly operable, effective, and can be promoted for use. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 : A structural schematic diagram of a 7 series aluminum alloy mold in the present invention;

[0029] Figure 2 : SEM image of a 7 series aluminum alloy mold in the present invention (the scale in the figure is 100μm). Description of the drawings:

[0031] 1- mold body; 2- diversion hole; 3- diversion bridge; 4- welding chamber; 41- primary welding chamber; 42- secondary welding chamber; 5- reinforcement structure; 6- mold core; 7- working belt. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is further described in detail with specific embodiments below.

[0033] The mold of 7 series aluminum alloy is prone to breakage during use. There are three main reasons: first, the degree of alloying of 7 series aluminum is high, the extrusion pressure is large, and the mold is under great pressure; second, the Zn content in 7 series aluminum alloy is high, and Zn penetrates into the mold steel, which will reduce the thermal fatigue strength of the mold and cause fatigue cracks in the mold under high temperature and high pressure cyclic stress; third, the high temperature viscosity of 7 series alloy is large, and the pulling force on the male head of the mold is large during extrusion. Therefore, the present invention improves the performance indicators of various aspects of the mold from the perspective of mold processing.

[0034] Nitriding, also known as nitriding, refers to a chemical heat treatment process in which active nitrogen atoms penetrate into the surface of a workpiece at a certain temperature. The purpose is to provide the hardness, wear resistance, corrosion resistance and fatigue strength of the workpiece surface. However, the existing nitriding treatment still has the following problems: First, the influence of high content of Zn atoms in 7 series aluminum alloy on the performance of the mold matrix is ​​not recognized. Studies have shown that Zn atoms in 7 series aluminum alloys will diffuse into the grain boundaries in the mold steel during the extrusion process. The melting temperature of Zn is 419.53℃, and the extrusion temperature is higher than the melting point of Zn. Zn on the grain boundary exists in liquid form, so it will destroy the continuity of the metal. Under the action of tensile stress, the mold is prone to cracking at the Zn-containing grain boundary, causing zinc embrittlement cracking. Secondly, it is unclear about the depth of Zn atoms in 7 series aluminum alloys diffusing into the mold. In addition, the nitriding process applies compressive stress to the mold, but it will dissipate over time. Therefore, the nitriding frequency and cycle of the mold are unclear, and the role of nitriding cannot be played well.

[0035] In order to solve the above problems, the first aspect of the present invention provides a method for improving the service life of a 7 series aluminum alloy mold, wherein the mold is a manifold mold, comprising:

[0036] Select forged steel as raw material for processing to obtain a mold;

[0037] The mold is subjected to normalizing and tempering treatments to make the hardness of the mold reach 44-48HRC, wherein the temperature of the normalizing treatment is 850-870°C, and the temperature of the tempering treatment is 600-620°C;

[0038] The mold is subjected to nitriding treatment, and the depth of the nitrided layer obtained by the nitriding treatment is 220 to 310 μm.

[0039] In the present invention, the material of the mold is screened, and forged steel becomes the first choice of mold material. Forged steel has higher strength than H13 hot working die steel, and the internal structure is dense, without segregation, and the structure and performance are relatively balanced, can withstand greater pressure, and has better fatigue resistance. At the same time, the heat treatment process of the mold is optimized, and a heat treatment method of normalizing combined with tempering is adopted, and the normalizing temperature is reduced by about 20°C and the tempering temperature is increased by about 30°C, which can improve the toughness of the mold, reduce the residual stress inside the mold, and then improve the tensile strength and yield strength of the mold, reduce the risk of cracks in the mold during use, and extend the service life of the mold. The depth of the nitriding layer is 220-310μm, which can fully isolate the Zn ions in the 7 series aluminum alloy from diffusing into the matrix of the mold, avoid the bridge position of the mold from breaking, and further extend its service life.

[0040] Preferably, the forging steel includes 45A steel, 35CrMoL steel, stainless steel, or 4Cr3Mo3SiV steel.

[0041] See also Figure 1 The forged steel is selected as the raw material for processing to obtain the mold, which includes:

[0042] Forged steel is selected as raw material for processing to obtain a mold body 1; the mold body 1 is provided with a diversion hole 2, a diversion bridge 3, a mold core 6, and a working belt 7;

[0043] A diverter hole 2 with a flared shape is provided on the die body 1, and the diameter of the diverter hole 2 gradually decreases from the inlet end to the outlet end. On the basis of ensuring an appropriate diverter ratio, the thickness of the diverter bridge 3 is increased as much as possible, so that the inlet of the diverter hole 2 is set in a flared shape, which can reduce shear deformation as much as possible and reduce the extrusion force.

[0044] Furthermore, the process of selecting forged steel as raw material for processing to obtain a mold further comprises:

[0045] A shunt bridge 3 and a welding chamber 4 are provided in the mold body 1, and a reinforcement structure 5 is provided at the bridge position of the shunt bridge 3 near one end of the welding chamber 4. The provision of the reinforcement structure 5 can protect the mold bridge position from damage. Even if cracks appear in the stainless steel welding layer during the use of the mold, it will not affect the mold bridge position. It is only necessary to repeatedly add new weak structures to the bridge position near the end of the primary welding chamber 41 after cracks appear in the stainless steel welding layer. In some preferred embodiments, the reinforcement structure 5 includes a stainless steel layer, and the arrangement of the reinforcement structure 5 includes but is not limited to welding. In some embodiments, the welding chamber 4 includes a primary welding chamber 41 and a secondary welding chamber 42, and specifically, a reinforcement structure 5 can be provided at the bridge position near one end of the primary welding chamber 41.

[0046] In the present invention, by designing the shape of the diverter hole 2 and setting the reinforcement structure 5, the structure of the mold is optimized, the structural strength of the diverter bridge 3 of the mold can be improved, and the service life of the mold is extended.

[0047] Preferably, the normalizing treatment includes three stages: heating, heat preservation and cooling. The mold is heated to 850-870°C, exemplarily 850°C, 855°C, 860°C, 865°C, 870°C, but not limited thereto, followed by heat preservation treatment for 12-24 hours, and finally cooling at a cooling rate of 35-45°C / h. Increasing the normalizing temperature will result in higher hardness and greater brittleness, while lowering the normalizing temperature will result in lower hardness and better toughness.

[0048] Preferably, the tempering treatment is 600-620°C, exemplarily 600°C, 605°C, 610°C, 615°C, 620°C, but not limited thereto, the tempering treatment time is 0.5-2h, and the cooling rate is 2-4°C / s. By controlling the tempering treatment temperature, time, cooling rate and number of tempering times, the hardness of the mold can be effectively controlled within the range of 44-48HRC, further improving the toughness of the mold and increasing its ability to withstand pressure and pulling force.

[0049] Furthermore, the tempering treatment is performed 2 to 5 times, preferably 3 to 4 times.

[0050] Preferably, the method further comprises nitriding the mold, wherein the gas introduced in the nitriding treatment is ammonia gas, and the temperature of the nitriding treatment is 500-560° C. Specifically, the mold is placed in a nitriding furnace and NH3 is introduced, and heated to 500-560° C. NH3 will undergo a decomposition reaction at this temperature: 2NH3→2〔N〕+3H2, and most of the decomposed nitrogen atoms will generate N2 gas, and a small amount of active nitrogen atoms will be absorbed by the mold surface and then diffuse into the workpiece. After a period of NH3 treatment, a nitrided layer of a certain depth can be obtained on the surface of the mold.

[0051] Preferably, the specific steps of the nitriding treatment include:

[0052] (1) nitriding the newly produced mold;

[0053] (2) A short bar of 7 series aluminum alloy was extruded for one cycle using a nitrided die;

[0054] (3) removing the nitrided layer formed by the nitriding treatment and re-performing the nitriding treatment;

[0055] (4) Repeat steps (2) and (3).

[0056] The nitriding treatment is a periodic operation, and the nitriding treatment is repeated only after the residual nitriding layer is removed after one cycle. After a period of use, the residual nitriding layer is removed and then a new nitriding treatment is continued, so that the Zn diffused in the nitriding layer can be removed before entering the mold matrix, thereby avoiding the influence of Zn ions on the mechanical properties of the mold, ensuring sufficient nitriding layer depth, and giving full play to the role of the nitriding layer. At the same time, new compressive stress can be continuously applied to the mold surface to improve its surface fatigue strength and increase the mold life to a new height, from the original 300kg / set of molds to 10T / set of molds, until the 7 series aluminum alloy profile size is out of tolerance and the mold is scrapped, which increases the mold life by as much as 30 times.

[0057] Preferably, the depth of the nitride layer obtained by the nitridation treatment is 220-310 μm, exemplified by 220 μm, 230 μm, 240 μm, 250 μm, 260 μm, 270 μm, 280 μm, 290 μm, 300 μm, and 310 μm, but not limited thereto.

[0058] Furthermore, the depth of the nitride layer obtained by the nitridation treatment is 220-240 μm, which improves the adhesion of the nitride layer on the mold substrate while ensuring the blocking effect on Zn ions, thereby preventing the nitride layer from falling off.

[0059] In some preferred embodiments, the nitriding treatment is performed twice, and the depth of the obtained nitriding layer reaches 130-150 μm by the first nitriding treatment, and the depth of the obtained nitriding layer reaches 220-240 μm by continuing the second nitriding treatment. If only one nitriding treatment is performed, the nitriding layer is thin, which is not enough to isolate the Zn ions from diffusing into the substrate, and the bridge position often breaks within 40 short rods of the mold extrusion. However, if the third nitriding treatment is continued, the nitriding layer will be too thick, which has obvious disadvantages, resulting in insufficient adhesion of the nitriding layer and easy falling off.

[0060] Furthermore, the cycle is to extrude 140 to 160 7 series aluminum alloy short bars using the die.

[0061] In the present invention, the material and structural design of the mold are combined with the processing technology, so that the service life of the mold is significantly increased, which is more than 30 times compared with before. In addition, the processing method is simple, highly operable, effective, and can be promoted for use.

[0062] The present invention will be further described below with specific embodiments:

[0063] Example 1

[0064] This embodiment provides a method for improving the service life of a 7 series aluminum alloy mold, wherein the mold is a manifold mold, comprising:

[0065] (1) Forging steel is selected as raw material for processing to obtain a split die mold;

[0066] (2) normalizing and tempering the manifold mold to make the hardness of the manifold mold reach 46HRC;

[0067] The normalizing process is as follows: heating to 860°C and then keeping the temperature for 18 hours, and finally cooling at a cooling rate of 45°C / h; then heating to 610°C for tempering treatment for 1.5 hours, and then cooling at a cooling rate of 3°C / s, and repeating three times.

[0068] (3) Performing nitriding treatment: placing the newly produced mold in a nitriding furnace, introducing NH3 into the furnace, heating to 530°C, and performing nitriding twice continuously. The depth of the nitriding layer obtained by the first nitriding treatment is 140 μm, and the thickness of the nitriding layer obtained after the second nitriding treatment is 220 μm;

[0069] (4) 160 7 series aluminum alloy short bars were extruded using the treated die, the nitrided layer was removed, and the bars were re-nitrided twice in succession according to the above operation, and repeated 100 times.

[0070] The surface of the nitride layer of the tap mold obtained in step (4) was observed by SEM microscopic morphology, and the results were as follows: Figure 2 As shown, EDS analysis was performed on the element content in the edge of the nitride layer and the substrate of the manifold mold, and the results are shown in Tables 1 and 2.

[0071] Table 1 Test results of the composition of the edge of the nitride layer

[0072] element Mass / % Atom / % C 15.94 38.29 N 6.66 13.74 O 5.94 10.72 V 0.99 0.56 Cr 5.46 3.03 Fe 64.76 33.52 Zn 0.30 0.13 total 100 100

[0073] Table 2 Test results of the matrix composition of the manifold mold

[0074] element Mass / % Atom / % N 0.53 2.07 Cr 5.38 5.66 Fe 94.09 92.27 Zn nd nd C nd nd V nd nd total 100 100

[0075] pass Figure 2 It can be seen that a nitride layer with a thickness of about 220 μm is formed on the substrate of the manifold mold through nitriding treatment. From the data in Tables 1 and 2, it can be seen that Zn atoms are detected in the nitride layer, while there are no Zn atoms in the substrate of the manifold mold, indicating that the nitride layer with a thickness of 230 μm can completely prevent Zn ions from diffusing into the substrate of the manifold mold, so that the manifold mold maintains its toughness and improves its service life.

[0076] Example 2

[0077] This embodiment provides a method for increasing the service life of a 7 series aluminum alloy mold, which is basically the same as that of embodiment 1, except that:

[0078] The normalizing process is to heat to 850°C for 24 hours, and finally cool at a cooling rate of 42°C / h; then heat to 600°C for tempering for 2 hours, and then cool at a cooling rate of 2.5°C / s, and repeat three times, the hardness of the manifold mold reaches 44HRC;

[0079] The thickness of the nitrided layer obtained after the second nitriding treatment is 240 μm.

[0080] Example 3

[0081] This embodiment provides a method for increasing the service life of a 7 series aluminum alloy mold, which is basically the same as that of embodiment 1, except that:

[0082] The normalizing process is to heat to 870°C and then keep the temperature for 20 hours, and finally cool at a cooling rate of 35°C / h; then heat to 620°C for tempering for 1.5 hours, and then cool at a cooling rate of 2.5°C / s, and repeat three times, the hardness of the manifold mold reaches 48HRC;

[0083] The thickness of the nitrided layer obtained after the second nitriding treatment is 230 μm.

[0084] Comparative Example 1

[0085] This comparative example provides a method for increasing the service life of a 7 series aluminum alloy mold, which is basically the same as Example 1, except that:

[0086] The normalizing process is to heat to 900°C for 18 hours and finally cool at a cooling rate of 45°C / h to make the hardness of the manifold mold reach 50HRC.

[0087] Comparative Example 2

[0088] This comparative example provides a method for increasing the service life of a 7 series aluminum alloy mold, which is basically the same as Example 1, except that:

[0089] The tempering process is to heat to 570°C for tempering treatment for 1.5 hours, then cool at a cooling rate of 3°C / s, and repeat three times to make the hardness of the manifold mold reach 49HRC.

[0090] Comparative Example 3

[0091] This comparative example provides a method for increasing the service life of a 7 series aluminum alloy mold, which is basically the same as Example 1, except that:

[0092] H13 steel is selected as the raw material for processing to obtain a diverter die.

[0093] Performance Testing

[0094] The tensile strength and impact toughness of the tap hole molds obtained in steps (3) and (4) of the embodiment and the comparative example were tested respectively. The results are shown in Table 3 below.

[0095] Table 3 Performance test results of the embodiments and comparative examples

[0096]

[0097] From the above results, it can be seen that the normalizing and tempering treatment procedures in the present invention, combined with a nitriding layer of a specific thickness, can significantly improve the tensile strength, yield strength and impact toughness of the 7 series aluminum alloy mold, thereby extending its service life, greatly saving mold costs, reducing product production costs, and improving market competitiveness.

[0098] The above disclosure is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.

Claims

1. A method for increasing the service life of a 7 series aluminum alloy mold, characterized in that: The mold is a diverter mold, comprising: Select forged steel as raw material for processing to obtain a mold; The mold is subjected to normalizing and tempering treatments to make the hardness of the mold reach 44-48HRC, wherein the temperature of the normalizing treatment is 850-870°C, and the temperature of the tempering treatment is 600-620°C; The mold is subjected to nitriding treatment, and the depth of the nitrided layer obtained by the nitriding treatment is 220 to 310 μm.

2. The method for increasing the service life of a 7 series aluminum alloy mold according to claim 1, characterized in that: The specific steps of the nitriding treatment include: (1) nitriding the newly produced mold; (2) A short bar of 7 series aluminum alloy was extruded for one cycle using a nitrided die; (3) removing the nitrided layer formed by the nitriding treatment and re-performing the nitriding treatment; (4) Repeat steps (2) and (3).

3. The method for increasing the service life of a 7 series aluminum alloy mold according to claim 1, characterized in that: The forging steel includes 45A steel, 35CrMoL steel, stainless steel, and 4Cr3Mo3SiV steel.

4. The method for increasing the service life of a 7 series aluminum alloy mold according to claim 1, characterized in that: The forged steel is selected as the raw material for processing to obtain the mold, which includes: Select forged steel as raw material for processing to obtain the mold body; A diverter hole with a flared shape is arranged on the mold body, and the diameter of the diverter hole gradually decreases from the inlet end to the outlet end.

5. The method for increasing the service life of a 7 series aluminum alloy mold according to claim 4, characterized in that: The process of selecting forged steel as raw material to obtain a mold further comprises: A shunt bridge and a welding chamber are arranged in the mold body. A reinforcement structure is arranged at a bridge position of the shunt bridge close to one end of the welding chamber, and the reinforcement structure includes a stainless steel layer.

6. The method for increasing the service life of a 7 series aluminum alloy mold according to claim 1, characterized in that: The holding time of the normalizing treatment is 12 to 24 hours, and the cooling rate is 35 to 45° C. / h. The tempering treatment time is 0.5 to 2 hours, the cooling rate is 2 to 4° C. / s, and the tempering treatment times are 2 to 5 times.

7. The method for increasing the service life of a 1-series aluminum alloy mold according to claim 1, characterized in that: The depth of the nitrided layer obtained by the nitridation treatment is 220-240 μm.

8. The method for increasing the service life of a 7 series aluminum alloy mold according to claim 7, characterized in that: The nitriding treatment is performed twice. The first nitriding treatment makes the depth of the obtained nitriding layer reach 130-150 μm. The second nitriding treatment is continued so that the depth of the obtained nitriding layer after the nitriding treatment reaches 220-240 μm.

9. The method for increasing the service life of a 7 series aluminum alloy mold according to claim 1, characterized in that: The gas introduced during the nitriding treatment is ammonia gas, and the temperature of the nitriding treatment is 500-560°C.

10. The method for increasing the service life of a 7 series aluminum alloy mold according to claim 2, characterized in that: The one cycle is to extrude 140 to 160 7 series aluminum alloy short bars using the die after nitriding treatment.

Citation Information

Patent Citations

  • Mold structure of large double-hole pipe profile with horizontal reinforcing ribs and processing method thereof

    CN103464502A

  • 7-class aluminum alloy large extrusion die

    CN104056869A

  • Graded-guiding multistage-splitting multiple-piece-combined complex-section mould

    CN110280721A

  • Surface composite treatment method for root of core of extrusion die

    CN112475822A

  • Die structure of high-strength large-section aluminum alloy template profile

    CN213728623U