Preparation method of ultra-high-purity tungsten filament
The 7N-grade ultra-high-purity tungsten plate prepared by chemical vapor deposition method is subjected to stress annealing and continuous heating-swaging treatment, which solves the problem of high impurity content of tungsten wire in the semiconductor field, realizes the preparation of high-purity tungsten wire, and improves its Purity and mechanical properties meet the needs of high-precision production.
Patent Information
- Application Number
- CN202410793758.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-06-19
AI Technical Summary
It is difficult to prepare high-purity tungsten wires that meet the requirements of the semiconductor ion implantation field with the existing technology. In particular, high-purity tungsten materials prepared by chemical vapor deposition are difficult to draw, which makes it difficult to reduce the content of impurity elements such as molybdenum, affecting device performance.
After stress annealing, the 7N-grade ultra-high-purity tungsten plate prepared by chemical vapor deposition method is processed by continuous heating, swaging and electrolytic polishing. The heating temperature and swaging compression ratio are controlled in stages, and gradually drawn into black tungsten wire. Finally, we obtain High purity tungsten wire.
The impurity content in the tungsten wire is significantly reduced, the purity and mechanical properties of the tungsten wire are improved, and the demand for high precision and efficiency in the semiconductor manufacturing field is met.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor high-purity materials, and in particular to a method for preparing ultra-high-purity tungsten wire. Background Art
[0002] In the frontier field of semiconductor technology, especially in the crucial process of ion implantation, there are very high requirements for the purity of the components used. This is because even trace amounts of impurities may have a profound impact on the performance of the final product. Among them, the purity of high-purity tungsten filaments, as one of the core components of ion implantation equipment, is strictly monitored and restricted. The reason why high-purity tungsten filaments are important is that they need to work stably under extreme conditions such as high temperature and high vacuum to provide a stable and efficient light source for ion implantation. However, impurity elements in the components, such as molybdenum, even at very small contents, may have a serious impact on the accuracy and efficiency of ion implantation, and thus affect the performance of semiconductor devices. Therefore, for the preparation of high-purity tungsten filaments, not only a high content of tungsten is required, but also an extremely low content of impurity elements. However, in nature, tungsten and molybdenum are common associated minerals, and their existence in the ore makes it difficult to completely separate the two during extraction and preparation. Although the existing powder metallurgy method for making tungsten has made significant progress in the extraction and purification of tungsten, it is still difficult to completely remove impurity elements such as molybdenum.
[0003] Among them, chemical vapor deposition (CVD) has attracted much attention due to its unique advantages. By precisely controlling the reaction conditions and selecting appropriate reactants, chemical vapor deposition can produce tungsten materials with extremely high purity. This method can not only effectively remove impurity elements such as molybdenum, but also ensure that the purity of tungsten meets the standards required in the semiconductor field. The tungsten material prepared by chemical vapor deposition is not only high in purity, but also has good crystallinity and organizational structure. This has significantly improved the physical and chemical properties of tungsten materials and can meet the semiconductor industry's demand for high-quality materials. By adjusting the reaction conditions, such as temperature, pressure, gas flow, etc., the deposition rate, film thickness and uniformity of tungsten can be precisely controlled. This makes chemical vapor deposition a reliable method for preparing high-quality tungsten materials. However, although tungsten materials prepared by chemical vapor deposition have many advantages, there are differences in the grain structure between high-purity tungsten products prepared by chemical vapor deposition and tungsten prepared by powder metallurgy (PM) process. CVD high-purity tungsten has a columnar crystal structure. Compared with the equiaxed crystal structure of PM tungsten, the columnar crystal structure has coarse grains and is very difficult to draw. The tungsten drawing process prepared by powder metallurgy (PM) cannot meet the drawing requirements of CVD high-purity tungsten.
[0004] In summary, most of the current tungsten wire drawing is based on tungsten prepared by powder metallurgy (PM), but the purity of the prepared tungsten wire does not meet the requirements of the ion implantation field. However, there is no relevant record of wire drawing of high-purity tungsten prepared by chemical vapor deposition (CVD). Therefore, it is urgent to propose a method for preparing ultra-high purity tungsten wire. Summary of the invention
[0005] In the prior art, tungsten prepared based on powder metallurgy (PM) is drawn, but the purity of the prepared tungsten wire does not meet the requirements of the ion implantation field. However, there is no relevant record of drawing high-purity tungsten prepared by chemical vapor deposition (CVD). Therefore, the present application proposes a method for preparing ultra-high-purity tungsten wire.
[0006] The technical solution of this application is as follows:
[0007] A method for preparing ultra-high purity tungsten wire comprises the following steps:
[0008] Step S1. Cutting an ultra-high purity tungsten rod with a diameter of 19 to 21 mm from an ultra-high purity tungsten plate;
[0009] Step S2. The ultra-high purity tungsten rod in step S1 is first subjected to high temperature heat treatment, and then subjected to continuous heating-rotary forging, and repeated heating-rotary forging to obtain a pretreated ultra-high purity tungsten rod;
[0010] Step S3. The ultra-high purity tungsten rod pretreated in step S2 is subjected to the processes of graphite emulsion, heating and wire drawing in sequence to obtain black tungsten wire, and the graphite emulsion, heating and wire drawing processes are repeated, followed by electrolytic polishing to obtain ultra-high purity tungsten wire.
[0011] Preferably, the ultra-high purity tungsten plate in step S1 is produced based on CVD technology, and its grain structure is a columnar crystal structure with a purity of 7N grade; the ultra-high purity tungsten plate needs to be stress annealed before use, the annealing temperature is 800-1200°C, the heating rate is 50-100°C / h, the insulation time is 5-10h, and then air-cooled; the ultra-high purity tungsten rod is cut by wire, and the length of the ultra-high purity tungsten rod is not less than 400mm.
[0012] Preferably, the annealing temperature is 900-1200° C., the heating rate is 60-80° C. / h, and the holding time is 7-10 h.
[0013] Preferably, the annealing temperature is 1050-1150° C., the heating rate is 65-75° C. / h, and the holding time is 9-10 h.
[0014] Preferably, the high temperature heat treatment parameters in step S2 are: a rising current rate of 1000-1100 A / min, a maximum current of 3800A-4200A, a holding time of 20-25 min, a falling current rate of 700-900 A / min, and air cooling for 25-30 min.
[0015] Preferably, the high temperature heat treatment parameters in step S2 are as follows: a rising current rate of 1030-1070 A / min, a maximum current of 4000 A-4100 A, a holding time of 23-25 min, and a falling current rate of 750-850 A / min.
[0016] Preferably, the high temperature heat treatment parameters in step S2 are: a rising current rate of 1050-1060 A / min, a maximum current of 4070 A-4100 A, a holding time of 24-25 min, and a falling current rate of 800-820 A / min.
[0017] Preferably, the heating-rotary forging in step S2 is divided into three stages: L1, L2, and L3 according to the diameter of the ultra-high purity tungsten rod.
[0018] Preferably, in the L1 stage, the diameter of the ultra-high purity tungsten rod is 13-20 mm, the heating temperature is 600-800° C., the heating time is 4-8 min, the rotary forging temperature is 550-750° C., the rotary forging forward speed is 3-5 m / min, and the tungsten rod rotary forging compression ratio is 10-18%.
[0019] Preferably, in the L1 stage, the heating temperature is 630-750° C., the heating time is 5-8 min, the rotary forging temperature is 600-700° C., the rotary forging forward speed is 3.5-4 m / min, and the tungsten rod rotary forging compression ratio is 12-16%.
[0020] Preferably, in the L1 stage, the heating temperature is 650-700° C., the heating time is 6-7 min, the rotary forging temperature is 630-670° C., the rotary forging forward speed is 3.5-3.8 m / min, and the tungsten rod rotary forging compression ratio is 13.5-14.5%.
[0021] Preferably, in the L2 stage, the diameter of the ultra-high purity tungsten rod is 7-13 mm, the heating temperature is 500-700° C., the heating time is 3-7 min, the rotary forging temperature is 450-650° C., the rotary forging forward speed is 3-5 m / min, and the tungsten rod rotary forging compression ratio is 10-18%.
[0022] Preferably, in the L2 stage, the heating temperature is 530-650° C., the heating time is 4-7 min, the rotary forging temperature is 500-600° C., the rotary forging forward speed is 3.5-4 m / min, and the tungsten rod rotary forging compression ratio is 12-16%.
[0023] Preferably, in the L2 stage, the heating temperature is 550-600° C., the heating time is 5-6 min, the rotary forging temperature is 530-570° C., the rotary forging forward speed is 3.5-3.8 m / min, and the tungsten rod rotary forging compression ratio is 13.5-14.5%.
[0024] Preferably, in the L3 stage, the diameter of the ultra-high purity tungsten rod is 4-7 mm, the heating temperature is 400-600° C., the heating time is 2-6 min, the rotary forging temperature is 350-550° C., the rotary forging forward speed is 3-5 m / min, and the tungsten rod rotary forging compression ratio is 12-20%.
[0025] Preferably, in the L3 stage, the heating temperature is 430-550° C., the heating time is 3-6 min, the rotary forging temperature is 400-500° C., the rotary forging forward speed is 3.5-4 m / min, and the tungsten rod rotary forging compression ratio is 15-17%.
[0026] Preferably, in the L3 stage, the heating temperature is 450-500° C., the heating time is 4-5 min, the rotary forging temperature is 430-470° C., the rotary forging forward speed is 3.5-3.8 m / min, and the tungsten rod rotary forging compression ratio is 15.5-16.5%.
[0027] Preferably, the wire drawing in step S3 is divided into three stages, P1, P2, and P3, according to the diameter of the high-purity tungsten rod. In the P1 stage, the diameter of the ultra-high purity tungsten rod is 2-4 mm, the wire drawing temperature is 420-450°C, and the wire drawing compression ratio is 17-23%; in the P2 stage, the diameter of the ultra-high purity tungsten rod is 1-2 mm, the wire drawing temperature is 400-430°C, and the wire drawing compression ratio is 18-24%; in the P3 stage, the diameter of the ultra-high purity tungsten rod is 0.5-1 mm, the wire drawing temperature is 380-410°C, and the wire drawing compression ratio is 19-25%.
[0028] Preferably, in the P1 stage in step S3, the wire drawing temperature is 430-440°C, and the wire drawing compression ratio is 19-21%; in the P2 stage, the wire drawing temperature is 410-420°C, and the wire drawing compression ratio is 20-22%; in the P3 stage, the wire drawing temperature is 390-400°C, and the wire drawing compression ratio is 21-23%.
[0029] Preferably, in the P1 stage in step S3, the wire drawing temperature is 432-435°C, and the wire drawing compression ratio is 19.5-20.5%; in the P2 stage, the wire drawing temperature is 412-415°C, and the wire drawing compression ratio is 20.5-21.5%; in the P3 stage, the wire drawing temperature is 392-395°C, and the wire drawing compression ratio is 21.5-22.5%.
[0030] Beneficial effects of this application:
[0031] (1) The high-purity tungsten wire preparation method proposed in this application uses a 7N grade ultra-high purity tungsten plate prepared by chemical vapor deposition (CVD) as raw material. This high-purity tungsten plate is in high demand in the field of semiconductor manufacturing, especially ion implantation. Compared with traditional tungsten wire, its impurity content is extremely low, which solves the problem of being unable to meet high-precision production requirements due to excessive impurities. At the same time, it also greatly reduces the potential harm of impurities to equipment, and improves overall production efficiency and product quality.
[0032] (2) The present application first subjects the ultra-high purity tungsten rod to high temperature heat treatment, using continuous heating-rotary forging, wherein the heating-rotary forging is divided into three stages, L1, L2, and L3, according to the diameter of the ultra-high purity tungsten rod. Key parameters such as temperature and time are set for each stage to ensure that the uniformity of the material and the stability of the performance are maintained as the diameter of the tungsten rod gradually decreases, thereby obtaining a high-purity tungsten rod. Subsequently, the present application performs fine wire drawing on the high-purity tungsten rod. According to the diameter of the tungsten rod, the wire drawing process is divided into three stages, P1, P2, and P3. In each stage, key parameters such as the wire drawing temperature and the wire drawing compression ratio are strictly controlled to ensure that the final tungsten wire has excellent performance. Not only does it ensure the purity and uniformity of the tungsten wire, but it also greatly improves its mechanical properties and stability. DETAILED DESCRIPTION
[0033] In order to further explain the technical means and effects adopted by the present application to achieve the predetermined invention purpose, the specific implementation method, structure, characteristics and effects of the present application are described in detail below in combination with the preferred embodiments.
[0034] Embodiments 1 to 5
[0035] This embodiment provides a method for preparing an ultra-high purity tungsten wire. It should be noted that the main difference between embodiments 1 to 5 lies in the different process parameters, as shown in Tables 1 to 3, which are as follows:
[0036] Step S1. An ultra-high purity tungsten plate with a columnar crystal structure produced based on CVD technology and a purity of 7N is stress annealed in a heat treatment furnace at an annealing temperature of 800-1200°C, a heating rate of 50-100°C / h, and a holding time of 5-10h. It is then air-cooled in the heat treatment furnace, and the ultra-high purity tungsten rod is cut by wire cutting until the surface is smooth and has no protrusions or depressions. The diameter of each ultra-high purity tungsten rod is controlled to be 19-21mm and the length is not less than 400mm.
[0037] By adopting the above annealing treatment, the stress generated inside the tungsten plate during the chemical vapor deposition production process can be effectively removed, and the wire drawing performance of the tungsten rod can be improved.
[0038] Step S2. The ultra-high purity tungsten rod in step S1 is first subjected to high temperature heat treatment by point vertical melting. The parameters of the electric hammer melting are as follows: the rising current rate is 1000-1100 / min, the maximum current is 3800-4000A, the insulation time is 20-25min, the falling current rate is 700-900A / min, and the electric hammer melting equipment is air-cooled for 25-30min.
[0039] Then, after continuous heating and rotary forging, it is divided into three stages, L1, L2 and L3, according to the diameter of the ultra-pure tungsten rod, and repeated heating and rotary forging to obtain a pre-treated ultra-high purity tungsten rod; wherein, in the L1 stage, when the diameter of the ultra-high purity tungsten rod is 13-20 mm, the heating temperature is 600-800°C, the heating time is 4-8 min, the rotary forging temperature is 550-750°C, the rotary forging forward speed is 3-5 m / min, and the tungsten rod rotary forging compression ratio is 10-18%. In the L2 stage, when the diameter of the ultra-high purity tungsten rod is 7-13 mm, the heating temperature is 500-700°C, the heating time is 3-7 min, the rotary forging temperature is 450-650°C, the rotary forging forward speed is 3-5 m / min, and the tungsten rod rotary forging compression ratio is 10-18%. In the L3 stage, when the diameter of the ultra-high purity tungsten rod is 4-7 mm, the heating temperature is 400-600°C, the heating time is 2-6 min, the rotary forging temperature is 350-550°C, the rotary forging forward speed is 3-5 m / min, and the tungsten rod rotary forging compression ratio is 12-20%.
[0040] By adopting the above technology, high temperature heat treatment is carried out by electric vertical melting, which can be controlled by current to provide a temperature higher than that of general heat treatment furnaces; high temperature heat treatment can further remove the internal stress of the tungsten rod so that it meets the requirements of rotary forging and wire drawing. The heating-rotary forging process is adopted in the ultra-pure tungsten rod. Heating can preheat the tungsten rod and improve the rotary forging performance of the tungsten rod. Rotary forging can effectively reduce the internal stress of the tungsten rod and improve the rotary forging performance of the tungsten rod.
[0041] Step S3. The ultra-high purity tungsten rod pretreated in step S2 is sequentially subjected to the process of attaching graphite emulsion, heating and drawing to obtain black tungsten wire, and the graphite emulsion, heating and drawing process are repeated until the diameter is 0.5-2 mm, and electrolytic polishing is performed to obtain ultra-high purity tungsten wire. Among them, the wire drawing is divided into three stages: P1, P2, and P3 according to the diameter of the high purity tungsten rod. In the P1 stage, the diameter of the ultra-high purity tungsten rod is 2-4 mm, the drawing temperature is 420-450°C, and the drawing compression ratio is 17-23%; in the P2 stage, the diameter of the ultra-high purity tungsten rod is 1-2 mm, the drawing temperature is 400-430°C, and the drawing compression ratio is 18-24%; in the P3 stage, the diameter of the ultra-high purity tungsten rod is 0.5-1 mm, the drawing temperature is 380-410°C, and the drawing compression ratio is 19-25%.
[0042] Table 1 Annealing parameters
[0043] sample Annealing temperature(℃) Heating rate (℃ / h) Insulation time (h) Example 1 1100 70 10 Example 2 1000 50 5 Example 3 800 80 7 Example 4 900 90 8 Example 5 1200 1000 9
[0044] Table 2 High heat treatment parameters
[0045]
[0046]
[0047] Table 3 L1 stage processing parameters
[0048]
[0049] Table 4 L2 stage processing parameters
[0050]
[0051] Table 5 L3 stage processing parameters
[0052]
[0053]
[0054] Table 6 Processing parameters of P1 to P3 stages
[0055]
[0056] After testing, the tungsten wire prepared by the method of this application has a purity of 7N grade and a diameter of 0.5 to 1 mm. This is because the raw material of the high-purity tungsten wire preparation method proposed in this application is a 7N grade ultra-high purity tungsten plate prepared by chemical vapor deposition (CVD). Compared with traditional tungsten wire, its impurity content is extremely low, which solves the problem that it cannot meet the high-precision production requirements due to excessive impurities. This application first performs high-temperature heat treatment on the ultra-high purity tungsten rod, and then uses continuous heating-rotary forging. Among them, heating-rotary forging is divided into three stages: L1, L2, and L3 according to the diameter of the ultra-high purity tungsten rod. Each stage sets key parameters such as temperature and time to ensure that the uniformity of the material and the stability of the performance of the tungsten rod are maintained during the gradual reduction of the diameter of the tungsten rod, and then the high-purity tungsten rod is finely drawn in this application. According to the size of the tungsten rod diameter, the wire drawing process is divided into three stages: P1, P2, and P3. In each stage, the key parameters such as the drawing temperature and the drawing compression ratio are strictly controlled to ensure that the final tungsten wire has excellent performance. It not only ensures the purity and uniformity of the tungsten wire, but also greatly improves its mechanical properties and stability.
[0057] The above is only a preferred embodiment of the present application and does not constitute any form of limitation to the present application. Although the present application has been disclosed as a preferred embodiment as above, it is not intended to limit the present application. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present application. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present application without departing from the content of the technical solution of the present application are still within the scope of the technical solution of the present application.
Claims
1. A method for preparing ultra-high purity tungsten wire, It is characterized in that The steps include: Step S1. Cutting an ultra-high purity tungsten rod with a diameter of 19 to 21 mm from an ultra-high purity tungsten plate; Step S2. The ultra-high purity tungsten rod in step S1 is first subjected to high temperature heat treatment, and then subjected to continuous heating-rotary forging, and repeated heating-rotary forging to obtain a pretreated ultra-high purity tungsten rod; Step S3. The ultra-high purity tungsten rod pretreated in step S2 is subjected to the processes of graphite emulsion, heating and wire drawing in sequence to obtain black tungsten wire, and the graphite emulsion, heating and wire drawing processes are repeated, followed by electrolytic polishing to obtain ultra-high purity tungsten wire.
2. The method for preparing an ultra-high purity tungsten wire according to claim 1, It is characterized in that The ultra-high purity tungsten plate in step S1 is produced based on CVD technology, and its grain structure is a columnar crystal structure with a purity of 7N grade; the ultra-high purity tungsten plate needs to be stress annealed before use, the annealing temperature is 800-1200°C, the heating rate is 50-100°C / h, the insulation time is 5-10h, and then air-cooled; the ultra-high purity tungsten rod is cut by wire, and the length of the ultra-high purity tungsten rod is not less than 400mm.
3. The method for preparing an ultra-high purity tungsten wire according to claim 1, It is characterized in that The high temperature heat treatment parameters in step S2 are as follows: a rising current rate of 1000-1100 A / min, a maximum current of 3800 A-4200 A, a holding time of 20-25 min, a falling current rate of 700-900 A / min, and air cooling of 25-30 min.
4. The method for preparing an ultra-high purity tungsten wire according to claim 1, It is characterized in that In step S2, the heating-rotation forging is divided into L according to the diameter of the ultra-high purity tungsten rod. 1 , L 2 , L 3 Three stages.
5. The method for preparing an ultra-high purity tungsten wire according to claim 4, It is characterized in that The L 1 In this stage, the diameter of the ultra-high purity tungsten rod is 13-20 mm, the heating temperature is 600-800°C, the heating time is 4-8 min, the rotary forging temperature is 550-750°C, the rotary forging forward speed is 3-5 m / min, and the tungsten rod rotary forging compression ratio is 10-18%.
6. The method for preparing an ultra-high purity tungsten wire according to claim 4, It is characterized in that The L 2 In this stage, the diameter of the ultra-high purity tungsten rod is 7-13 mm, the heating temperature is 500-700°C, the heating time is 3-7 min, the rotary forging temperature is 450-650°C, the rotary forging forward speed is 3-5 m / min, and the tungsten rod rotary forging compression ratio is 10-18%.
7. The method for preparing an ultra-high purity tungsten wire according to claim 4, It is characterized in that The L 3 In this stage, the diameter of the ultra-high purity tungsten rod is 4-7 mm, the heating temperature is 400-600°C, the heating time is 2-6 min, the rotary forging temperature is 350-550°C, the rotary forging forward speed is 3-5 m / min, and the tungsten rod rotary forging compression ratio is 12-20%.
8. The method for preparing an ultra-high purity tungsten wire according to claim 1, It is characterized in that In step S3, the wire drawing is divided into P according to the diameter of the high-purity tungsten rod. 1 , P 2 , P 3 Three stages, P 1 In the first stage, the diameter of the ultra-high purity tungsten rod is 2-4 mm, the drawing temperature is 420-450°C, and the drawing compression ratio is 17-23%; 2 In the first stage, the diameter of the ultra-high purity tungsten rod is 1-2 mm, the drawing temperature is 400-430°C, and the drawing compression ratio is 18-24%; 3 In this stage, the diameter of the ultra-high purity tungsten rod is 0.5-1mm, the drawing temperature is 380-410℃, and the drawing compression ratio is 19-25%.
Citation Information
Patent Citations
Saw for cutting silicon into seed rods for use in chemical vapor deposition polysilicon reactor
CN103813891A
Preparation method of high-purity tungsten target material
CN114457319A
Tungsten alloy wire and preparation method thereof
CN114855046A
Preparation method of high-strength superfine tungsten alloy wire for cutting
CN114888292A
Method for manufacturing tungsten workpiece for secondary working
JP2004243416A