Leather dyeing process
By using chemicals such as acetate, synthetic retanning agents and formates in the leather dyeing process to adjust the pH value and fiber structure of the leather, the problem of insufficient color fastness of cowhide is solved and higher color fastness is achieved and softness.
Patent Information
- Application Number
- CN202410936579.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-25
AI Technical Summary
The color fastness of existing cowhide is difficult to meet people's needs, especially in terms of dye adsorption and fixation capabilities.
A leather dyeing process that includes retanning, rinsing, alkaline, core, capping and fatliquoring steps to condition the leather through the use of acetates, synthetic retanning agents, formates, leather softeners and fixatives The pH value and fiber structure ensure adequate fixation and even distribution of the dye.
The color fastness and softness of dyed cowhide are improved, making it more durable, light-resistant, and heat-resistant during use, while maintaining a good appearance and feel.
Smart Images

Figure BDA0004941501040000091 
Figure BDA0004941501040000101 
Figure BDA0004941501040000102
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of leather production, and in particular to a leather dyeing process. Background Art
[0002] Leather, especially genuine leather, refers to animal skin that has been denatured and is not easy to rot after physical and chemical processing such as depilation and tanning. The animal skin is composed of natural protein fibers tightly woven in three-dimensional space. Its surface has a special grain layer with natural grain and luster, and feels comfortable. After dyeing, leather can be obtained into colorful leather products to meet people's visual needs.
[0003] Among them, the absorption and fixation ability of cowhide to dye is relatively low, thus affecting the color fastness of leather. Now as people's needs continue to increase, the existing color fastness of cowhide can no longer meet people's needs. Summary of the invention
[0004] In order to solve the problem that the color fastness of existing cowhide can no longer meet people's needs, the present application provides a new leather dyeing process. The dyed cowhide produced by this dyeing process has higher color fastness and softness than the existing dyed cowhide.
[0005] In a first aspect, the present application provides a leather dyeing process, which adopts the following technical solution: A leather dyeing process comprises the following steps: Retanning: The cowhide is reacted with a polymer and then transferred into a retanning mixture consisting of a synthetic melamine resin and a dispersant to react to obtain retanned cowhide; Rinsing: adding the retanned cowhide to a rinsing mixture consisting of a surfactant and a degreasing agent for reaction, then transferring to an oxalic acid solution for reaction, and washing with water to obtain rinsed cowhide; Alkali extraction: adding the rinsed cowhide to an alkali extraction mixed solution composed of acetate and synthetic retanning agent for reaction, and then transferring to a formate solution for reaction to obtain alkali extracted cowhide; Core penetration: reacting the alkali-extracted cowhide with a leveling agent solution, and then transferring it into a leather dye for reaction to obtain core penetration cowhide; Covering: reacting the core penetration cowhide with a cover leather dye, and then transferring it into a cover leather fixative for reaction to obtain cover cowhide; Fatliquoring: adding the cover cowhide to a leather softener for reaction, then transferring it to a first leather fixer for reaction, and then adding it to a second leather fixer for reaction to obtain fatliquored cowhide; Drying: the fatliquored cowhide is washed and dried to obtain dyed cowhide.
[0006] By adopting the above technical solution, acetate plays a role in adjusting the pH value during the alkali extraction process. By soaking the leather in a mixture containing acetate, the pH value of the leather can be reduced, that is, its acidity can be increased. This is to ensure that the subsequent dyeing process can proceed smoothly, because some dyes need to be better fixed and penetrated into the leather under specific acidic conditions; Synthetic retanning agents are mainly used to further fix the fiber structure of leather in the alkali extraction step and improve the tanning effect of leather. By reacting with leather fibers, synthetic retanning agents can enhance the durability, softness and water resistance of leather; formate solution further adjusts the pH value of leather in the alkali extraction step to ensure that the leather is in the best dyeing state; formate can also enhance the light resistance and heat resistance of leather, making it less likely to change color or be damaged during use; Leather softener is mainly used to improve the softness and feel of leather. By adding softener, the fiber structure in the leather can be relaxed, making it softer and more comfortable, and giving the leather a unique luster and texture; The first leather fixative is mainly used to fix the dyes and softeners in the leather, ensuring that they will not fall off or fade easily during use. The fixative can also enhance the wear resistance and durability of the leather, making it more durable; The second leather fixative is usually a reinforcing agent used to further enhance the fixing effect of the leather. By deeply reacting with the leather fibers, the second fixative can provide more lasting protection, allowing the leather to maintain its good appearance and performance when affected by external forces or environmental factors; The present application adds acetate, synthetic retanning agent and formate solution during alkali extraction, and adds leather softener, first leather fixative and second leather fixative during fatliquoring. Through their mutual cooperation, the dye is fully fixed in the leather, so that the dyed cowhide produced by this dyeing process has higher color fastness and softness than the existing dyed cowhide.
[0007] Preferably, in the alkali extraction step, when the rinsed cowhide reacts with the alkali extraction mixed solution, the temperature of the rinsed cowhide and the alkali extraction mixed solution is 32-37°C.
[0008] By adopting the above technical solution, different dyes and auxiliaries have different solubility at different temperatures; controlling the temperature within the range of 32-37°C helps to ensure good dissolution of dyes and auxiliaries in the mixed solution, thereby improving their reaction efficiency and uniformity with leather; Leather is a heat-sensitive material. Excessively high temperatures may damage and shrink leather fibers, causing leather deformation or uneven color. Controlling the reaction temperature at 32-37°C can avoid such heat damage and maintain the integrity and texture of the leather. The speed of chemical reactions usually increases with increasing temperature; however, too high a temperature may cause the reaction to be too fast and difficult to control; choosing 32-37°C as the reaction temperature can ensure the reaction efficiency while giving the operator enough time to monitor and adjust the reaction progress.
[0009] Preferably, in the alkali extraction step, the concentration of the formate is 0.6-1.0 wt %, and the reaction time of the rinsed cowhide transferred to the formate solution is 35-45 min.
[0010] By adopting the above technical solution, the main purpose of the alkali extraction step is to adjust the pH value of the leather to promote the subsequent dyeing process; formate, as an acidic substance, reacts with the alkaline substances in the rinsed cowhide to neutralize, thereby adjusting the pH value of the leather to a suitable dyeing range; the concentration is controlled at 0.6-1.0wt% to ensure that the speed and degree of the acid-base neutralization reaction are moderate, neither too fast to make the reaction difficult to control, nor too slow to affect production efficiency; Appropriate formate concentration and good reaction time help the dye to better penetrate into the leather fibers and ensure uniform dyeing; at an appropriate concentration, formate can increase the solubility and diffusion rate of the dye, making it evenly distributed in the leather fibers; If the concentration of formate is too high or the reaction time is too long, the leather may be over-treated, resulting in a hard texture or too dark color. On the contrary, if the concentration is too low or the reaction time is too short, the desired dyeing effect may not be achieved. Therefore, controlling the concentration at 0.6-1.0wt% and the reaction time at 35-45 minutes can ensure that the leather is properly treated.
[0011] Preferably, in the alkali extraction step, the pH range of the formate solution is 5.3-5.7.
[0012] By adopting the above technical solution, within this pH range, formate can effectively react with the alkaline substances in the rinsed cowhide to neutralize the leather, and adjust the pH value of the leather to a suitable range; this pH value can ensure that the speed of the neutralization reaction is moderate, and will not be too fast to cause leather damage, nor too slow to affect production efficiency; The pH value of leather has an important influence on the subsequent dyeing process; controlling the pH value within the range of 5.3-5.7 helps the dye to better combine with the leather fiber and improve the uniformity and fastness of the dyeing; pH value also has an important influence on the physical properties and chemical stability of leather; controlling the pH value within the range of 5.3-5.7 can ensure that the leather maintains good softness, wear resistance and weather resistance during the dyeing process.
[0013] Preferably, in the step of fatliquoring, the concentration range of the first leather fixer is 0.65-0.75 wt %, and the reaction time of the cover cowhide being transferred into the first leather fixer is 8-12 min.
[0014] By adopting the above technical solution, the main function of the leather fixative is to enhance the bonding force between leather fibers and improve the wear resistance and durability of the leather; the concentration is controlled within the range of 0.65-0.75wt%, which can ensure that the fixative is fully combined with the leather fibers to form a stable cross-linking structure, thereby effectively improving the physical properties of the leather; The setting of reaction time is crucial to the bonding effect between the fixative and the leather fibers. If the reaction time is too short, the fixative may not fully penetrate into the leather fibers, resulting in weak bonding. If the reaction time is too long, it may cause the leather to over-harden, affecting its softness and feel. Therefore, setting the reaction time to 8-12 minutes can ensure that the fixative fully reacts with the leather fibers while avoiding over-treatment. By controlling the concentration and reaction time of the fixative, it is possible to ensure that the leather maintains good softness, toughness and wear resistance after fatliquoring.
[0015] Preferably, in the step of fatliquoring, the concentration of the second leather fixer is in the range of 0.75-0.85 wt %, and the reaction time of the cover cowhide being transferred into the second leather fixer is 25-35 min.
[0016] By adopting the above technical solution, the second leather fixing agent may have stronger fixing performance than the first leather fixing agent; by increasing the concentration of the fixing agent to 0.75-0.85wt%, the degree of cross-linking between leather fibers can be further enhanced, thereby improving the wear resistance, crease resistance and chemical stability of the leather; Properly increasing the concentration of the fixative can help it better penetrate into the internal structure of the leather and react with more fibers; this will not only enhance the overall performance of the leather, but also ensure the uniformity and consistency of the inner and outer layers of the leather; The reaction time is extended from 8-12 minutes for the first fixing agent to 25-35 minutes for the second fixing agent to ensure that the second fixing agent has enough time to fully react with the leather fibers; a longer reaction time helps the fixing agent to be more evenly distributed in the leather and form a more stable cross-linked structure.
[0017] Preferably, in the step of fatliquoring, the pH of the second leather fixing agent is in the range of 3.3-3.7.
[0018] By adopting the above technical scheme, the leather fixing agent generally contains chemical groups that can react with functional groups on leather fibers; under acidic conditions (pH 3.3-3.7), these chemical groups may be more active and thus can be more effectively combined with leather fibers; Under a proper acidic environment, the reaction between the leather fixative and the leather fibers may be more complete and uniform, thereby improving the fixing effect; this helps to enhance the physical properties of the leather, such as wear resistance, crease resistance and dimensional stability; pH has an important influence on the quality and performance of leather; too high a pH value may cause the leather to over-swell and deform, while too low a pH value may destroy the natural structure of the leather; therefore, controlling the pH value within the range of 3.3-3.7 helps ensure that the leather maintains its original structure and quality during processing.
[0019] In summary, this application has the following beneficial effects: 1. Since the present application adds acetate, synthetic retanning agent and formate solution during alkali extraction, and adds leather softener, first leather fixative and second leather fixative during fatliquoring, the dye is fully fixed in the leather through their mutual cooperation, so that the dyed cowhide produced by this dyeing process has higher color fastness and softness than the existing dyed cowhide. DETAILED DESCRIPTION
[0020] The raw materials in this application include the following parts: Polymer: SELLATAN FL produced by Hebei Derui Chemical Co., Ltd. Synthetic melamine resin: synthetic melamine resin R7 produced by LANXESS Chemical (China) Co., Ltd.; Dispersant: Dispersant AU12 from Ningbo Modern Fine Chemical Co., Ltd. is used; Surfactant: Use surfactant from Hebei Derui Chemical Co., Ltd. SAF; Degreasing agent: Use high-efficiency degreasing agent AN-C from LANXESS Chemical (China) Co., Ltd.; Oxalic acid: a commercially available product with CAS number 144-62-7 was used; Acetate: A commercially available sodium acetate product with a CAS number of 6505-45-9 is used. A variety of acetate products can be selected in this application, such as sodium acetate, potassium acetate, lead acetate, etc. This application uses sodium acetate as an example for description; Synthetic retanning agent: SELLASOL NG, a synthetic retanning agent produced by Hebei Derui Chemical Co., Ltd. Formate: A commercially available sodium formate product with a CAS number of 141-53-7 is used. A variety of formate products can be selected in this application, such as sodium formate, potassium formate, lead formate, etc. This application uses sodium formate as an example for description; Leveling agent: non-ionic leveling agent AU08 from Ningbo Modern Fine Chemical Co., Ltd. is used; Leather dye: A new environmentally friendly leather dye from Ningbo Modern Fine Chemical Co., Ltd. is used. The leather dyes involved in the following examples are all this dye, and the only difference between different leather dyes is the concentration; Leather fixative: The leather fixative of Sinopharm Group is used. The leather fixatives involved in the following embodiments are all this fixative, and different leather fixatives only have different concentrations; Leather softener: Use leather softener DX-1202 from Hebei Derui Chemical Co., Ltd.; The present application is further described in detail below in conjunction with embodiments and comparative examples.
[0021] Example 1 A leather dyeing process comprises the following steps: Retanning: reacting the cowhide with a polymer for 60 min at a reaction temperature of 35°C and a polymer concentration of 10 wt%, and then transferring the mixture into a retanning solution composed of a synthetic melamine resin R7 and a dispersant AU12 for reaction for 60 min, wherein the concentration of the synthetic melamine resin R7 in the retanning solution is 3.0 wt% and the concentration of the dispersant AU12 is 1.5 wt%, to obtain retanned cowhide; Rinsing: adding the retanned cowhide to a rinsing mixture consisting of a surfactant and a degreasing agent to react for 90 minutes at a reaction temperature of 45°C, wherein the concentration of the surfactant in the rinsing mixture is 3.0wt%, and the concentration of the degreasing agent is 1.0wt%, and then transferring to an oxalic acid solution to react for 30 minutes, wherein the concentration of the oxalic acid is 0.3wt%, and washing with water twice to obtain rinsed cowhide; Alkali extraction: adding the rinsed cowhide to an alkali extraction mixture consisting of sodium acetate and a synthetic retanning agent to react for 20 minutes, the reaction temperature is 35°C, the concentration of sodium acetate in the alkali extraction mixture is 2.5wt%, the concentration of the synthetic retanning agent is 2.5wt%, and then transferring to a sodium formate solution to react for 40 minutes, the concentration of the sodium formate solution is 0.8wt%, and the pH of the sodium formate solution is 5.5, to obtain alkali-extracted cowhide; core penetration: reacting the alkali-extracted cowhide with a leveling agent solution for 10 minutes, the concentration of the leveling agent solution is 1.5wt%, and then transferring to a leather dye to react for 60 minutes, the concentration of the leather dye is 5.0wt%, to obtain core penetration cowhide; Covering: reacting the core leather with the cover leather dye for 10 min at a reaction temperature of 55° C., with the concentration of the cover leather dye being 1.5 wt %, and then transferring to the cover leather fixative to react for 40 min at a reaction temperature of 50° C. to obtain the cover leather; Fatliquoring: adding the cowhide to a leather softener with a concentration of 10.0wt% to react for 60 minutes, then transferring to a first leather fixer with a concentration of 0.7wt% to react for 10 minutes, then adding to a second leather fixer with a concentration of 0.8wt% to react for 30 minutes, and obtaining fatliquored cowhide; Drying: The fatliquored cowhide is washed and dried to obtain dyed cowhide.
[0022] Example 2-3 In Example 2-3, based on the preparation method of Example 1, the temperature of the rinsing cowhide and the alkali extraction mixed solution during the reaction is adjusted, and the specific adjustment is shown in Table 1.
[0023] Comparative Example 1-2 Comparative Example 1-2 is based on the preparation method of Example 1, and the temperature of the rinsing cowhide and the alkali extraction mixed solution during the reaction is adjusted. The specific adjustment is shown in Table 1.
[0024] Comparative Example 3 Commercially available dyed cowhide.
[0025] Table 1 Alkali extraction reaction temperature and performance test table of Examples 1-3 and Comparative Examples 1-3 project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Alkali extraction temperature / ℃ 35 32 37 30 40 / Color fastness / grade 5-6 4-5 5 3-4 4 4-5 Tensile strength / MPa 30.2 22.6 26.1 17.8 20.5 23.1 Elongation at break / % 60.3 50.7 57.2 42.3 46.6 50.3 Performance Test The dyed cowhides of Examples 1-3 and Comparative Examples 1-3 were subjected to the following performance tests, and the test results are shown in Table 1: 1. Color fastness According to the measurement method described in QB / T2537-2001 "Leather - Colour fastness test - reciprocating friction colour fastness", the colour is graded using the GB251 Grey Scale for Staining, with the higher the rating, the better.
[0026] 2. Softness The tensile strength and elongation at break are tested in accordance with the national standard "QB / T2710-2005 Physical and Mechanical Tests of Leather - Determination of Tensile Strength and Elongation". The higher the tensile strength and elongation at break, the better.
[0027] Referring to Table 1, by comparing Examples 1-3 and Comparative Examples 1-3, it can be seen that compared with Comparative Example 3, the color fastness, tensile strength and elongation at break of Examples 1 and 3 are higher than those of Comparative Example 3, and the color fastness, tensile strength and elongation at break of Example 2 and Comparative Example 3 are similar, indicating that the dyed cowhide of the present application has higher color fastness and softness than the existing dyed cowhide; as the alkali extraction reaction temperature continues to increase, the color fastness, tensile strength and elongation at break of the dyed cowhide show a trend of first increasing and then decreasing, which may be because as the alkali extraction reaction temperature continues to increase, it helps to ensure the good dissolution of dyes and auxiliaries in the mixed solution, improve their reaction efficiency and uniformity with leather, thereby improving the color fastness and softness of the dyed cowhide; when it exceeds a certain range, it may cause damage and shrinkage of leather fibers, causing leather deformation or uneven color, thereby reducing the color fastness and softness of the dyed cowhide.
[0028] Embodiment 4-5 Example 4-5 Based on the preparation method of Example 1, the concentration of sodium formate was adjusted, and the specific adjustment is shown in Table 2.
[0029] Comparative Examples 4-5 Comparative Example 4-5 Based on the preparation method of Example 1, the concentration of sodium formate was adjusted, and the specific adjustment is shown in Table 2.
[0030] The dyed cowhides of Example 4-5 and Comparative Example 4-5 were subjected to the above performance tests, and the test results are shown in Table 2.
[0031] Table 2 Sodium formate concentration and performance test table of Example 1, Example 4-5 and Comparative Example 4-5 project Example 1 Example 4 Example 5 Comparative Example 4 Comparative Example 5 Sodium formate / wt% 0.8 0.6 1.0 0.4 1.2 Color fastness / grade 5-6 23.7 27.4 18.6 21.1 Tensile strength / MPa 30.2 52.1 58.2 43.5 47.4 Elongation at break / % 60.3 4-5 5 3-4 4 Referring to Table 2, by comparing Example 1, Examples 4-5 and Comparative Example 4-5, it can be seen that as the concentration of sodium formate continues to increase, the color fastness, tensile strength and elongation at break of the dyed cowhide show a trend of first increasing and then decreasing. This may be because as the concentration of sodium formate continues to increase, the dye helps to better penetrate into the leather fibers and ensure the uniformity of dyeing, thereby improving the color fastness and softness of the dyed cowhide; when it exceeds a certain range, it may lead to excessive processing of the leather, causing the leather texture to become hard or the color to be too dark, reducing the color fastness and softness of the dyed cowhide.
[0032] Embodiment 6-7 In Example 6-7, based on the preparation method of Example 1, the reaction time of transferring the rinsed cowhide into the sodium formate solution was adjusted, and the specific adjustment is shown in Table 3.
[0033] Comparative Examples 6-7 Comparative Example 6-7 is based on the preparation method of Example 1, and the reaction time of transferring the rinsed cowhide into the sodium formate solution is adjusted. The specific adjustment is shown in Table 3.
[0034] The dyed cowhides of Example 6-7 and Comparative Example 6-7 were subjected to the above performance tests, and the test results are shown in Table 3.
[0035] Table 3. Reaction time and performance test table of rinsed cowhide of Example 1, Example 6-7 and Comparative Example 6-7 project Example 1 Example 6 Example 7 Comparative Example 6 Comparative Example 7 Reaction time / min 40 35 45 30 50 Color fastness / grade 5-6 4-5 5 3-4 4 Tensile strength / MPa 30.2 23.3 26.8 18.3 20.7 Elongation at break / % 60.3 51.6 57.7 43.0 46.9 Referring to Table 3, it can be seen from the comparison of Example 1, Examples 6-7 and Comparative Examples 6-7 that, as the reaction time of the rinsed cowhide being transferred to the sodium formate solution continues to increase, the color fastness, tensile strength and elongation at break of the dyed cowhide show a trend of first increasing and then decreasing. This may be because as the reaction time of the rinsed cowhide being transferred to the sodium formate solution continues to increase, the dye helps to better penetrate into the leather fibers and ensure the uniformity of dyeing, thereby improving the color fastness and softness of the dyed cowhide; when it exceeds a certain range, it may lead to excessive processing of the leather, causing the leather texture to become hard or the color to be too dark, reducing the color fastness and softness of the dyed cowhide.
[0036] Embodiment 8-9 Example 8-9 Based on the preparation method of Example 1, the pH of the sodium formate solution was adjusted, and the specific adjustment is shown in Table 4.
[0037] Comparative Examples 8-9 Comparative Examples 8-9 Based on the preparation method of Example 1, the pH of the sodium formate solution was adjusted, and the specific adjustment is shown in Table 4.
[0038] The dyed cowhides of Examples 8-9 and Comparative Examples 8-9 were subjected to the above performance tests, and the test results are shown in Table 4.
[0039] Table 4 pH and performance test table of sodium formate solution of Example 1, Examples 8-9 and Comparative Examples 8-9 project Example 1 Example 8 Example 9 Comparative Example 8 Comparative Example 9 Sodium formate solution pH 5.5 5.3 5.7 5.1 5.9 Color fastness / grade 5-6 4-5 5 3-4 4 Tensile strength / MPa 30.2 22.4 26.5 17.5 20.2 Elongation at break / % 60.3 50.4 57.5 41.9 46.2 Referring to Table 4, it can be seen from the comparison of Example 1, Examples 8-9 and Comparative Examples 8-9 that, as the pH of the sodium formate solution continues to increase, the color fastness, tensile strength and elongation at break of the dyed cowhide show a trend of first increasing and then decreasing. This may be because as the pH of the sodium formate solution continues to increase, the dye helps to better combine with the leather fibers, thereby improving the color fastness and softness of the dyed cowhide; when it exceeds a certain range, it may cause leather damage, reducing the color fastness and softness of the dyed cowhide.
[0040] Embodiment 10-11 Examples 10-11 Based on the preparation method of Example 1, the concentration of the first leather fixing agent was adjusted, and the specific adjustments are shown in Table 5.
[0041] Comparative Examples 10-11 Comparative Examples 10-11 Based on the preparation method of Example 1, the concentration of the first leather fixing agent was adjusted, and the specific adjustment is shown in Table 5.
[0042] The dyed cowhides of Examples 10-11 and Comparative Examples 10-11 were subjected to the above performance tests, and the test results are shown in Table 5.
[0043] Table 5 Concentration and performance test table of the first leather fixing agent of Example 1, Examples 10-11 and Comparative Examples 10-11 Referring to Table 5, it can be seen from the comparison of Example 1, Examples 10-11 and Comparative Examples 10-11 that, as the concentration of the first leather fixative continues to increase, the color fastness, tensile strength and elongation at break of the dyed cowhide show a trend of first increasing and then decreasing. This may be because as the concentration of the first leather fixative continues to increase, the first leather fixative and the leather fibers are gradually and fully combined to form a stable cross-linked structure, thereby improving the color fastness and softness of the dyed cowhide; when it exceeds a certain range, it may cause the dye to excessively penetrate into the leather, reducing the color fastness and softness of the dyed cowhide.
[0044] Examples 12-13 In Examples 12-13, based on the preparation method of Example 1, the reaction time of transferring the cowhide cover into the first leather fixing agent was adjusted. The specific adjustments are shown in Table 6.
[0045] Comparative Examples 12-13 Comparative Examples 12-13 are based on the preparation method of Example 1, and the reaction time of transferring the cover cowhide into the first leather fixing agent is adjusted. The specific adjustments are shown in Table 6.
[0046] The dyed cowhides of Examples 12-13 and Comparative Examples 12-13 were subjected to the above performance tests, and the test results are shown in Table 6.
[0047] Table 6 Reaction time and performance test table of cover cowhide transferred into the first leather fixing agent of Example 1, Examples 12-13 and Comparative Examples 12-13 project Example 1 Example 12 Example 13 Comparative Example 12 Comparative Example 13 First reaction / min 10 8 12 6 14 Color fastness / grade 5-6 4-5 5 4 4 Tensile strength / MPa 30.2 24 26.7 20.2 21.5 Elongation at break / % 60.3 52.5 57.7 45.8 48.0 Referring to Table 6, it can be seen from the comparison of Example 1, Examples 12-13 and Comparative Examples 12-13 that, as the reaction time of the cover cowhide being transferred into the first leather fixative continues to increase, the color fastness, tensile strength and elongation at break of the dyed cowhide show a trend of first increasing and then decreasing. This may be because as the reaction time of the cover cowhide being transferred into the first leather fixative continues to increase, the first leather fixative gradually penetrates into the leather fibers, thereby improving the color fastness and softness of the dyed cowhide; when it exceeds a certain range, it may cause the leather to harden excessively, reducing the color fastness and softness of the dyed cowhide.
[0048] Examples 14-15 Examples 14-15 Based on the preparation method of Example 1, the concentration of the second leather fixing agent was adjusted, and the specific adjustments are shown in Table 7.
[0049] Comparative Examples 14-15 Comparative Examples 14-15 Based on the preparation method of Example 1, the concentration of the second leather fixing agent was adjusted, and the specific adjustments are shown in Table 7.
[0050] The dyed cowhides of Examples 14-15 and Comparative Examples 14-15 were subjected to the above performance tests, and the test results are shown in Table 7.
[0051] Table 7 Concentration and performance test table of the second leather fixing agent of Example 1, Examples 14-15 and Comparative Examples 14-15 Referring to Table 7, it can be seen from the comparison of Example 1, Examples 14-15 and Comparative Examples 14-15 that, as the concentration of the second leather fixative continues to increase, the color fastness, tensile strength and elongation at break of the dyed cowhide show a trend of first increasing and then decreasing. This may be because as the concentration of the second leather fixative continues to increase, the degree of cross-linking between the leather fibers can be further enhanced, thereby improving the color fastness and softness of the dyed cowhide; when it exceeds a certain range, it may cause excessive hardening of the leather, reducing the color fastness and softness of the dyed cowhide.
[0052] Examples 16-17 In Examples 16-17, based on the preparation method of Example 1, the reaction time of transferring the cover cowhide into the second leather fixing agent was adjusted. The specific adjustments are shown in Table 8.
[0053] Comparative Examples 16-17 Comparative Examples 16-17 are based on the preparation method of Example 1, and the reaction time of transferring the cover cowhide into the second leather fixing agent is adjusted. The specific adjustments are shown in Table 8.
[0054] The dyed cowhides of Examples 16-17 and Comparative Examples 16-17 were subjected to the above performance tests, and the test results are shown in Table 8.
[0055] Table 8 Reaction time and performance test table of cover cowhide transferred into the second leather fixing agent of Example 1, Examples 16-17 and Comparative Examples 16-17 Referring to Table 8, it can be seen from the comparison of Example 1, Examples 16-17 and Comparative Examples 16-17 that, with the increasing reaction time of the cover cowhide being transferred into the second leather fixative, the color fastness, tensile strength and elongation at break of the dyed cowhide show a trend of first increasing and then decreasing. This may be because as the reaction time of the cover cowhide being transferred into the second leather fixative continues to increase, the second leather fixative is helped to be more evenly distributed in the leather, forming a more stable cross-linked structure, thereby improving the color fastness and softness of the dyed cowhide; when it exceeds a certain range, it may cause the leather to harden excessively, reducing the color fastness and softness of the dyed cowhide.
[0056] Examples 18-19 Examples 18-19 Based on the preparation method of Example 1, the pH of the second leather fixing agent was adjusted. The specific adjustment is shown in Table 9.
[0057] Comparative Examples 18-19 Comparative Examples 18-19 Based on the preparation method of Example 1, the pH of the second leather fixing agent was adjusted, and the specific adjustment is shown in Table 9.
[0058] The dyed cowhides of Examples 18-19 and Comparative Examples 18-19 were subjected to the above performance tests, and the test results are shown in Table 9.
[0059] Table 9 pH and performance test table of the second leather fixing agent of Example 1, Examples 18-19 and Comparative Examples 18-19 Referring to Table 9, it can be seen from the comparison of Example 1, Examples 18-19 and Comparative Examples 18-19 that, as the pH of the second leather fixative continues to increase, the color fastness, tensile strength and elongation at break of the dyed cowhide show a trend of first increasing and then decreasing. This may be because as the pH of the second leather fixative continues to increase, the reaction between the leather fixative and the leather fibers may be more sufficient and uniform, thereby improving the fixing effect, thereby improving the color fastness and softness of the dyed cowhide; when it exceeds a certain range, it may cause excessive expansion and deformation of the leather, reducing the color fastness and softness of the dyed cowhide.
[0060] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A leather dyeing process, characterized in that: The following steps are involved: Retanning: The cowhide is reacted with a polymer and then transferred into a retanning mixture consisting of a synthetic melamine resin and a dispersant to react to obtain retanned cowhide; Rinsing: adding the retanned cowhide to a rinsing mixture consisting of a surfactant and a degreasing agent for reaction, then transferring to an oxalic acid solution for reaction, and washing with water to obtain rinsed cowhide; Alkali extraction: adding the rinsed cowhide to an alkali extraction mixed solution composed of acetate and synthetic retanning agent for reaction, and then transferring to a formate solution for reaction to obtain alkali extracted cowhide; Core penetration: reacting the alkali-extracted cowhide with a leveling agent solution, and then transferring it into a leather dye for reaction to obtain core-penetrating cowhide; Covering: reacting the core-penetrating cowhide with a cover leather dye, and then transferring the cover leather fixative to react to obtain the cover cowhide; Fatliquoring: adding the cover cowhide to a leather softener for reaction, then transferring it to a first leather fixer for reaction, and then adding it to a second leather fixer for reaction to obtain fatliquored cowhide; Drying: the fatliquored cowhide is washed and dried to obtain dyed cowhide.
2. The leather dyeing process according to claim 1, characterized in that: In the alkali extraction step, when the rinsed cowhide reacts with the alkali extraction mixed solution, the temperature of the rinsed cowhide and the alkali extraction mixed solution is 32-37°C.
3. The leather dyeing process according to claim 2, characterized in that: In the alkali extraction step, the concentration of the formate is 0.6-1.0 wt %.
4. The leather dyeing process according to claim 3, characterized in that: In the alkali extraction step, the reaction time of the rinsed cowhide transferred to the formate solution is 35-45 minutes.
5. The leather dyeing process according to claim 3, characterized in that: In the alkali extraction step, the pH range of the formate solution is 5.3-5.
7.
6. The leather dyeing process according to claim 1, characterized in that: In the fatliquoring step, the concentration of the first leather fixing agent is in the range of 0.65-0.75 wt %.
7. The leather dyeing process according to claim 6, characterized in that: In the step of fatliquoring, the reaction time of the cover cowhide being transferred into the first leather fixing agent is 8-12 minutes.
8. The leather dyeing process according to claim 1, characterized in that: In the fatliquoring step, the concentration of the second leather fixing agent is in the range of 0.75-0.85 wt %.
9. The leather dyeing process according to claim 8, characterized in that: In the step of fatliquoring, the reaction time of the cover cowhide being transferred into the second leather fixing agent is 25-35 minutes.
10. The leather dyeing process according to claim 8, characterized in that: In the fatliquoring step, the pH of the second leather fixing agent is in the range of 3.3-3.7.
Citation Information
Patent Citations
Leather dyeing process
CN118308542A