Method for efficiently extracting lithium by compounding ammonium sulfate with low-temperature roasted lepidolite

Through the low-temperature roasting process of mixed salts of ammonium sulfate and persulfate and activated lepidolite, the problem of high-temperature roasting and complex leaching in the lithium extraction process of lepidolite is solved, achieving efficient and low-energy lithium ion extraction and ensuring a high leaching rate. and environmental protection.

CN118835103APending Publication Date: 2024-10-25JIANGXI YONGXING SPECIAL STEEL NEW ENERGY TECH CO LTD +1
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202411055300.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

In the existing lithium extraction process from lepidolite, the roasting temperature is high and the leaching process is complicated, resulting in high energy consumption and cost, and increased volatilization of harmful elements.

Method used

A mixed salt of ammonium sulfate and persulfate is mixed with activated lepidolite. Through pre-heating and low-temperature roasting, mechanical activation and ammonium sulfate decomposition are used to promote the reaction of lepidolite, lower the roasting temperature and increase the reaction rate, and combine with water to leach lithium.

Benefits of technology

It achieves high-efficiency extraction of lithium at low temperatures, reduces energy consumption and costs, ensures that the lithium ion leaching rate is above 90%, reduces the volatilization of harmful elements, and the process is simple.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118835103A_ABST
    Figure CN118835103A_ABST
Patent Text Reader

Abstract

The method comprises the following steps: pretreating a lepidolite raw material to obtain lepidolite concentrate, and treating the lepidolite concentrate in a mechanical activation manner to obtain activated lepidolite concentrate; an auxiliary material and the activated lepidolite concentrate are evenly mixed according to the material ratio of 1.2 g / g-1. 6 g / g, a mixed material is obtained, and the auxiliary material is mixed salt of ammonium sulfate and persulfate; roasting equipment is preheated to 650-750 DEG C, the mixed material is put into the roasting equipment to be roasted, and lepidolite roasted clinker A is obtained; and the lepidolite roasting clinker A is subjected to water leaching and mechanical oscillation to obtain a lithium-containing leachate. The method is simple in technological process, the adopted sulfate mixture is low in price, the temperature required by roasting is far lower than that of a traditional method, energy consumption is low, meanwhile, efficient leaching of lithium is guaranteed, cost is greatly reduced, and the method has wide application prospects in the field of lithium extraction through lepidolite roasting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical smelting, and relates to a method for efficiently extracting lithium from ammonium sulfate-compounded low-temperature roasted lepidolite. Background Art

[0002] Lepidolite is one of the main raw materials for preparing battery-grade lithium carbonate. At present, the lithium extraction process of lepidolite covers a variety of methods such as pressure cooking, chlorination, and sulfate roasting. Yichun, Jiangxi Province has rich lepidolite resources. After long-term development, the lithium extraction process of lepidolite in this area is mainly based on sulfate roasting.

[0003] At present, the methods for roasting lithium mica sulfate are as follows: In the Chinese patent "A method for extracting lithium from lithium mica to prepare lithium carbonate" (CN202210826237.X), lithium mica is mixed with concentrated sulfuric acid, sulfate and calcium compound for multiple times and roasted at 850-950℃, and then water-leached at 50-70℃ to obtain lithium sulfate leachate. In the Chinese patent "A new method for preparing lithium carbonate by roasting lithium mica" (CN202111063039.4), lithium mica is mixed with sodium potassium sulfate mixed salt, auxiliary agent and calcium carbonate, and the mixture is granulated and sent to a rotary kiln, roasted at 850-900℃, and then water-leached to obtain lithium sulfate mother liquor, and then lithium carbonate is obtained through a series of impurity removal, evaporation and concentration of sodium carbonate. In the Chinese patent "A process for preparing lithium carbonate by roasting lithium mica sulfate" (CN202310137498.5), the lithium mica is first crushed and mixed with potassium sulfate, calcium oxide, etc. at 115-130°C for 2-3 hours, and then the mixture is placed in a rotary kiln and roasted at 850-900°C, and an extractant composed of chlorocyclohexane acid, modified isooctyl alcohol, and sulfonated kerosene is selected to extract lithium from the clinker. In the Chinese patent "A method for recycling lithium extraction from lithium mica and lithium carbonate prepared therefrom" (CN202211734747.0), the lithium mica and calcium sulfate are roasted at 950-1100°C and then leached to extract lithium.

[0004] The sulfates used in the above patents are mainly traditional sodium potassium salts, and the roasting temperatures are relatively high. Some methods select acid leaching or selective extraction in the leaching step, and the leaching process is complicated. Therefore, if the roasting temperature can be reduced while ensuring the lithium leaching rate and a convenient leaching method can be used, energy consumption and costs can be greatly reduced. Summary of the invention

[0005] The purpose of the present invention is to solve the deficiencies of the prior art, and thus a method for efficiently extracting lithium from lepidolite by low-temperature roasting of ammonium sulfate is proposed. The method is to simply mechanically activate the lepidolite concentrate, mix it evenly with auxiliary materials (mixed salt of ammonium sulfate and persulfate), and roast it by pre-heating and then setting out, thereby reducing the loss of auxiliary materials during the heating process, effectively reducing the temperature required for roasting, and ensuring the leaching rate of lithium. The present invention has the advantages of simple operation, low energy consumption, and low auxiliary material cost.

[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions: A method for efficiently extracting lithium from ammonium sulfate-compounded low-temperature calcined lepidolite comprises the following steps: The lepidolite raw material is pretreated to obtain lepidolite concentrate, the lepidolite concentrate is mechanically activated to obtain activated lepidolite concentrate, auxiliary materials and the activated lepidolite concentrate are uniformly mixed at a material ratio of 1.2g / g-1.6g / g to obtain a mixed material, wherein the auxiliary material is a mixed salt of ammonium sulfate and persulfate; a roasting device is preheated to 650-750°C, and the mixed material is placed in the device for roasting to obtain lepidolite roasted clinker A; and the lepidolite roasted clinker A is subjected to water immersion and mechanical vibration to obtain a lithium-containing leachate.

[0007] Furthermore, the persulfate is one or more of potassium persulfate, sodium persulfate, potassium persulfate, ammonium persulfate, and ammonium persulfate.

[0008] Furthermore, the persulfate is one or both of sodium persulfate and potassium persulfate.

[0009] Furthermore, the lepidolite concentrate is placed in an oven for drying before activation.

[0010] Furthermore, the mass ratio of sulfate to persulfate in the auxiliary material is 1:1.

[0011] Furthermore, the mechanical activation method is ball milling, the ball milling speed is 400-600rpm, and the ball milling time is 60-90min.

[0012] Furthermore, the method further comprises: the activated lepidolite concentrate is passed through a 60-80 mesh sieve before roasting.

[0013] Furthermore, the calcination temperature is 700°C.

[0014] Furthermore, the calcination time is 60-140 min, preferably 80-120 min, and more preferably 100 min.

[0015] Furthermore, the mechanical oscillation time is 40-60 minutes.

[0016] Furthermore, the water immersion temperature is 30-90°C.

[0017] In the above technical solution, the pretreatment of the lithium mica ore mainly includes crushing, impurity removal, drying and other processes.

[0018] In the above technical solution, the roasting equipment can be a muffle furnace or a box furnace.

[0019] Principle of the present invention: The present invention increases the specific surface area of ​​lepidolite by mechanical activation treatment, provides more active sites, thereby improving the reactivity of lepidolite with sulfate, and further accelerating the reaction rate. In addition, mechanical activation can also destroy the lattice structure of lepidolite, and inject additional energy into the crystal structure through the strain and thermal effects introduced by collision and friction, resulting in irregular changes in its structure. These changes may cause dislocations and defects in the crystal structure of lepidolite, reduce its activation energy, thereby enhancing chemical activity, and enabling lepidolite to effectively react with sulfate at a lower temperature.

[0020] The present invention introduces low-melting-point ammonium sulfate and persulfate, and the mixed salt changes the phase equilibrium of the mineral during the reaction process, which may lead to the emergence of the system eutectic point, further reducing the melting point of the system. In addition, during the roasting process, the decomposition of ammonium sulfate releases ammonia, which increases the looseness and porosity of the mineral particles, is conducive to the contact between the auxiliary materials and the inside of the mineral, and helps to adjust the pH value of the reaction environment, thereby affecting the solubility of the mineral. At the same time, the decomposition of ammonium sulfate can also produce sulfur dioxide, etc., and persulfate can produce free radicals. Sulfur dioxide may directly participate in the reaction process of lithium mica, and the generated free radicals can also promote the decomposition of minerals such as lithium mica. Therefore, adding a mixed salt of ammonium sulfate and persulfate changes the reaction path, and at the same time affects the lattice structure of lithium mica, resulting in lattice distortion or energy reduction, which is conducive to realizing the decomposition of minerals and the release of lithium at a lower temperature. The mixed salt of ammonium sulfate and persulfate used in the present invention shows a synergistic effect, which can promote the destruction of the lithium mica structure at a lower temperature and effectively exchange lithium ions. By utilizing the water solubility of lithium sulfate, lithium can be efficiently extracted by simple water immersion.

[0021] Beneficial effects of the present invention: The process for efficiently extracting lithium from lepidolite by low-temperature roasting of ammonium sulfate compounded with the present invention has simple operation steps, relatively low price of the mixed salt auxiliary material used, and low roasting temperature required for roasting, which greatly reduces energy consumption. Meanwhile, the reduction of roasting temperature can reduce the volatilization of harmful elements (such as thallium, etc.), and ensures that the leaching rate of lithium ions is above 90% under the premise of considering environmental protection and energy consumption cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 This is a trend diagram of lithium leaching rate at different roasting temperatures in Example 1 of the present invention.

[0024] Figure 2 This is a trend diagram of lithium leaching rate at different roasting times in Example 2 of the present invention.

[0025] Figure 3 This is a trend chart of lithium leaching rate under different types of auxiliary materials in Example 8 of the present invention. DETAILED DESCRIPTION

[0026] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments.

[0028] In the examples, unless otherwise specified, all means used are conventional means in the art, and all raw materials used are commercially available conventional products.

[0029] Example 1: This example compares the lithium leaching rate of lepidolite and ammonium sulfate auxiliary materials at different roasting temperatures. The specific implementation process is as follows: First, the lithium mica ore is pretreated to obtain lithium mica concentrate, and the concentrate is placed in an 80°C oven for drying. Ammonium sulfate and the dried lithium mica concentrate are evenly mixed in a mass ratio of 1.4:1, and then placed in a quartz crucible and placed in a muffle furnace. The muffle furnace roasting temperatures are set to 500°C, 650°C, 600°C, 700°C, 750°C, and 800°C, respectively, and the insulation time is 100 minutes. After the roasting is completed, the roasted lithium mica clinker is taken out when the temperature cools to room temperature, and the lithium mica clinker is poured into a conical flask, and a certain amount of pure water is injected. After sealing, it is oscillated at a constant temperature of 25°C, and then taken out after oscillation for 60 minutes, and filtered through a Buchner funnel to obtain a lithium-containing leachate. The lithium ion leaching rate in the leachate is analyzed by ICP-OES. The specific results are as follows Figure 1 shown.

[0030] analyze Figure 1 It can be seen from the results that the leaching rate at 700°C is much higher than that at other roasting temperatures, reaching 60%.

[0031] Example 2: This example compares the lithium leaching rate of lepidolite and ammonium sulfate auxiliary material at different roasting times. The specific implementation process is as follows: First, the lithium mica ore is pretreated to obtain lithium mica concentrate, and the concentrate is placed in an oven at 80°C for drying and standby use. Ammonium sulfate and the dried lithium mica concentrate are evenly mixed in a mass ratio of 1.4:1, and then placed in a quartz crucible and placed in a muffle furnace. The muffle furnace roasting temperature is set to 700°C, and the insulation time is 60min, 80min, 100min, 120min, and 140min, respectively. After the roasting is completed, when the temperature is cooled to room temperature, the roasted lithium mica clinker is taken out, poured into a conical flask, and a certain amount of pure water is injected. After sealing, it is oscillated at a constant temperature of 25°C, taken out after oscillation for 60min, and filtered through a Buchner funnel to obtain a lithium-containing leachate. The lithium ion leaching rate in the leachate is analyzed by ICP-OES. The specific results are as follows Figure 2 shown.

[0032] analyze Figure 2 The results show that the lithium leaching rate is the highest when the roasting time is 100 minutes. This may be because the roasting time is too long, causing the lithium to form a new mineral structure or be coated by other mineral structures.

[0033] Example 3: This example compares the leaching rate of lithium before and after mechanical activation of lepidolite. The specific implementation process is as follows: First, the lithium mica ore is pretreated to obtain lithium mica concentrate, and two portions of the concentrate are placed in an 80°C oven for drying. One portion of the lithium mica concentrate is ball milled at a speed of 500rpm and mechanically activated for 60min. Ammonium sulfate is mixed with the activated and unactivated concentrates at a mass ratio of 1.4:1 to obtain mixtures A and B, wherein A is the activated concentrate mixture and B is the unactivated concentrate mixture. Subsequently, the activated A mixture and B mixture are placed in a quartz crucible and placed in a muffle furnace, and the muffle furnace roasting temperature is set to 700°C for a constant holding time of 100min. After the roasting is completed, the roasted lithium mica clinker A and B are taken out when the temperature is cooled to room temperature, and the lithium mica clinker A and B are poured into a conical flask respectively, a certain amount of pure water is injected, and a constant temperature of 25°C is kept after sealing for oscillation. After 60min of oscillation, it is taken out and filtered through a Buchner funnel to obtain lithium-containing leachates A and B. The lithium ion leaching rate in the leaching solution was analyzed by ICP-OES, and the specific results are shown in Table 1.

[0034] Table 1

[0035] From the analysis of the results in Table 1, it can be seen that the leaching rate of the mixed material after mechanical activation has been greatly improved, reaching 87.35%.

[0036] Example 4: The present invention compares the lithium leaching rate of lithium mica mixed with different types of sulfates at a roasting temperature of 700° C. after ball milling. The specific implementation process is as follows: First, the lithium mica ore is pretreated to obtain lithium mica concentrate, and the concentrate is ball-milled at a speed of 500rpm and mechanically activated for 60min. The activated lithium mica concentrate is mixed with sodium sulfate or ammonium sulfate at a mass ratio of 1:1.4 to obtain two groups of mixed materials. Then the mixture is placed in a quartz crucible and placed in a muffle furnace, and the muffle furnace roasting temperature is set to 700℃ constant, and the insulation time is 100min. After the roasting is completed, the roasted lithium mica clinker is taken out when the temperature is cooled to room temperature, and the lithium mica clinker is poured into a conical flask, and a certain amount of pure water is injected. After sealing, it is oscillated at a constant temperature of 25℃, and then taken out after oscillation for 60min, and filtered through a Buchner funnel to obtain a lithium-containing leachate. The lithium ion leaching rate in the leachate is analyzed by ICP-OES, and the specific results are shown in Table 2.

[0037] Table 2

[0038] From the analysis of the results in Table 2, it can be seen that different types of sulfates have a significant contrast in the effect on the leaching rate of lithium. When calcined under the same conditions at a temperature of 700°C, the leaching rate of lithium in the sodium sulfate system is less than 20%, while that in the ammonium sulfate system reaches 87.35%.

[0039] Example 5: This example compares the lithium leaching rate under different placement methods during the roasting process. The specific implementation process is as follows: First, the lithium mica ore is pretreated to obtain lithium mica concentrate, and the concentrate is placed in an 80℃ oven for drying. The concentrate is ball-milled at a speed of 500rpm and mechanically activated for 60min. The activated lithium mica concentrate and ammonium sulfate are mixed evenly at a mass ratio of 1:1.4 and placed in a muffle furnace for roasting. The roasting methods are direct roasting (roasting at 700℃ for 100min), staged roasting (roasting at 500℃ for 60min and then heating to 700℃ for 40min), and preheating and then roasting (referring to heating to the specified temperature of 700℃ and then putting the mixed material into the roasting, and the roasting time is 100min). After the roasting is completed, the lithium mica clinker is taken out when it is cooled to room temperature, and the lithium mica clinker is poured into a conical flask, a certain amount of pure water is injected, and it is sealed and shaken at a constant temperature of 25℃. After 60min of oscillation, it is taken out and filtered through a Buchner funnel to obtain a lithium-containing leachate. The lithium ion leaching rate in the leaching solution was analyzed by ICP-OES, and the specific results are shown in Table 3.

[0040] Table 3

[0041] From the results of Table 3, it can be seen that the leaching rate of roasted lithium is the highest, which is 90.13%, in the preheating and then sampling mode.

[0042] Example 6: The present invention compares the lithium leaching rate of lithium mica mixed with different types of persulfates at a roasting temperature of 700° C. after ball milling. The specific implementation process is as follows: First, the lithium mica ore was pretreated to obtain lithium mica concentrate, and the concentrate was ball-milled at a speed of 500rpm and mechanically activated for 60min. The activated lithium mica concentrate was mixed with sodium persulfate, ammonium persulfate, and potassium persulfate in a mass ratio of 1:1.4 to obtain three groups of mixed materials, and then the mixed materials were placed in a quartz crucible and placed in a muffle furnace. The muffle furnace was set to a constant roasting temperature of 700℃ and the insulation time was 100min. After the roasting was completed, the roasted lithium mica clinker was taken out when the temperature was cooled to room temperature, and the lithium mica clinker was poured into a conical flask, a certain amount of pure water was injected, and the sealed flask was shaken at a constant temperature of 25℃. After 60min of shaking, it was taken out and filtered through a Buchner funnel to obtain a lithium-containing leachate. The lithium ion leaching rate in the leachate was analyzed by ICP-OES, and the specific results are shown in Table 4.

[0043] Table 4

[0044] From the analysis of the results in Table 4, it can be seen that different types of sulfates have a significant contrast in the effect on the leaching rate of lithium. When calcined under the same conditions at a temperature of 700°C, the leaching rate of lithium in the sodium persulfate system is 78.63%, the leaching rate of the ammonium persulfate system is 83.61%, and the leaching rate of the potassium persulfate system is 84.6%.

[0045] Example 7: This example compares the effect of water immersion temperature change on lithium leaching rate. The specific implementation process is as follows: First, the lithium mica ore was pretreated to obtain lithium mica concentrate, and the concentrate was placed in an 80℃ oven for drying. The dried concentrate was ball milled at a speed of 500rpm and mechanically activated for 60min. The activated lithium mica concentrate was mixed with ammonium sulfate and potassium persulfate in a mass ratio of 1:0.7:0.7 to obtain a mixture, and then the muffle furnace roasting temperature was set to 700℃ and the insulation time was 100min. After the muffle furnace temperature rose to 700℃, high-temperature rapid sampling was performed. After the roasting was completed, the roasted lithium mica clinker was taken out when the temperature cooled to room temperature, and the lithium mica clinker was poured into a conical flask, a certain amount of pure water was injected, and the sealed flask was immersed in water and oscillated in a constant temperature oscillating box. The immersion temperature was set to 30℃, 60℃ and 90℃ respectively. After oscillation for 60min, it was taken out and filtered through a Buchner funnel to obtain a lithium-containing leachate. The lithium ion leaching rate in the leachate was analyzed by ICP-OES, and the specific results are shown in Table 5.

[0046] Table 5

[0047] From the analysis of the results in Table 5, it can be seen that the leaching rate is improved to 96.2% when the immersion temperature is 90°C.

[0048] Example 8: The present invention compares the lithium leaching rate of lithium mica mixed with different mixed salt auxiliary materials at a roasting temperature of 700°C and after ball milling. The specific implementation process is as follows: First, the lithium mica ore was pretreated to obtain lithium mica concentrate, and the concentrate was ball-milled at a speed of 500rpm and mechanically activated for 60min. Ammonium sulfate and the activated lithium mica concentrate were mixed evenly in a mass ratio of 1.4:1 to obtain mixture 1; the activated lithium mica concentrate was mixed evenly with ammonium sulfate and ammonium persulfate in a mass ratio of 1:0.7:0.7 to obtain mixture 2; the activated lithium mica concentrate was mixed evenly with ammonium sulfate and potassium persulfate in a mass ratio of 1:0.7:0.7 to obtain mixture 3, and then the muffle furnace roasting temperature was set to 700℃ and the insulation time was constant for 100min. After the muffle furnace temperature rose to 700℃, high-temperature rapid lofting was carried out. After the roasting is completed, when the temperature is cooled to room temperature, the two groups of roasted lithium mica clinkers are taken out, poured into a conical bottle, a certain amount of pure water is injected, sealed and oscillated in a constant temperature oscillation box, the water immersion temperature is set to 90°C and oscillated for 60 minutes, then taken out and filtered through a Buchner funnel to obtain a lithium-containing leachate. The lithium ion leaching rate in the leachate is analyzed by ICP-OES. The specific results are as follows: Figure 3 shown.

[0049] analyze Figure 3Compared with the leaching rate of ammonium sulfate alone after roasting, the effect of persulfate mixed salt is obvious. When roasted under the same conditions, the leaching rate of lithium in the ammonium sulfate plus ammonium persulfate system is 93.61%, and the ammonium sulfate plus potassium persulfate system reaches 96.2%, both higher than the pure ammonium sulfate roasting system.

[0050] The above-mentioned embodiments only express several implementation modes of the present invention, and the description thereof is relatively specific and detailed, but it should not be understood as limiting the scope of the invention patent.

[0051] It should be noted that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for efficiently extracting lithium from ammonium sulfate-compounded low-temperature calcined lepidolite, characterized in that: The following steps are involved: The lepidolite raw material is pretreated to obtain lepidolite concentrate, and the lepidolite concentrate is mechanically activated to obtain activated lepidolite concentrate; auxiliary materials and the activated lepidolite concentrate are uniformly mixed at a material ratio of 1.2g / g-1.6g / g to obtain a mixed material, wherein the auxiliary material is a mixed salt of ammonium sulfate and persulfate; a roasting device is preheated to 650-750°C, and the mixed material is placed in the device for roasting to obtain lepidolite roasted clinker A; and the lepidolite roasted clinker A is subjected to water immersion and mechanical vibration to obtain a lithium-containing leachate.

2. The process for efficiently extracting lithium from ammonium sulfate-compounded low-temperature calcined lepidolite according to claim 1, characterized in that: The persulfate is one or more of potassium hydrogen persulfate, sodium persulfate, potassium persulfate, ammonium persulfate, and ammonium hydrogen persulfate.

3. The process for efficiently extracting lithium from ammonium sulfate-compounded low-temperature calcined lepidolite according to claim 1, characterized in that: The mechanical activation method is ball milling; the ball milling speed is 400-600rpm, and the ball milling time is 60-90min.

4. The process for efficiently extracting lithium from ammonium sulfate-compounded low-temperature calcined lepidolite according to claim 1, characterized in that: The activated lepidolite concentrate is passed through a 60-80 mesh sieve before roasting.

5. The process for efficiently extracting lithium from ammonium sulfate-compounded low-temperature calcined lepidolite according to claim 1, characterized in that: The mass ratio of sulfate to persulfate in the auxiliary material is 1:

1.

6. The process for efficiently extracting lithium from ammonium sulfate-compounded low-temperature calcined lepidolite according to claim 1, characterized in that: The calcination temperature is 700°C.

7. The process for efficiently extracting lithium from ammonium sulfate-compounded low-temperature calcined lepidolite according to claim 1, characterized in that: The calcination time is 60-140 minutes.

8. The process for efficiently extracting lithium from ammonium sulfate-compounded low-temperature calcined lepidolite according to claim 1, characterized in that: The mechanical shaking time is 40-60 min.

9. The process for efficiently extracting lithium from ammonium sulfate-compounded low-temperature calcined lepidolite according to claim 1, characterized in that: The water immersion temperature is 30-90°C.

Citation Information

Cited By

  • Method for reducing roasting temperature of lepidolite and cooperatively extracting lithium, rubidium, cesium and potassium

    CN119979871A

  • Method for extracting lithium from lithium-containing resource

    CN120041683A

  • A method for extracting lithium from lithium-containing resources

    CN120041683B

  • Lithium extraction method for automatically controlling roasting process of lepidolite concentrate

    CN120843846A

  • Method for extracting lithium from spodumene acid through microwave and ultrasonic wave synergistic enhancement

    CN121380605A