Evaporation device, solar cell and preparation method of solar cell
By adjusting the gas partial pressure and flow rate through the evaporation device, the deposition method of the fullerene material is controlled, which solves the problem of controlling the morphology of the fullerene material in the existing technology and improves the performance and efficiency of organic electronic devices.
Patent Information
- Application Number
- CN202410851335.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-25
AI Technical Summary
It is difficult to effectively control the morphology of fullerene materials with existing technology, which affects the performance and efficiency of organic electronic devices, especially the interface morphology between the electron transport layer and the light-emitting layer or active layer.
An evaporation device is designed. By adjusting the gas generator and flow controller, the gas partial pressure and flow rate in the reaction chamber are adjusted, and the deposition method of the fullerene material is controlled to achieve the layered or island-like growth of the functional film layer. Thereby adjusting the shape of the electron transport layer.
By adjusting the gas content and partial pressure, precise control of the morphology of the functional film layer is achieved, which improves the surface stability and device performance of the electron transport layer, and improves the photoelectric conversion efficiency of organic electronic devices.
Smart Images

Figure CN118835201A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of coating devices, and in particular to an evaporation device, a solar cell and a method for preparing the same. Background Art
[0002] The electron transport layer is a key functional material in organic light-emitting diodes, organic photovoltaics, organic transistors and other organic electronic devices. It is mainly used to promote the efficient transport of electrons from the cathode to the light-emitting layer or active layer, thereby improving the performance and efficiency of the device.
[0003] In the prior art, fullerene is generally used as the electron transport layer material, and fullerene materials have large parasitic absorption. Therefore, in order to obtain high-performance organic electronic devices, vacuum evaporation is generally used to control the film thickness at the sub-nanometer level. The interface morphology of fullerene and the light-emitting layer or active layer significantly affects the defect recombination process of organic electronic devices. For this defect recombination process, the prior art research focuses more on adding interface passivation materials, replacing fullerene materials, etc., but lacks control over the intrinsic material morphology of fullerene materials. Summary of the invention
[0004] The purpose of the present application is to provide a vapor deposition device, a solar cell and a method for preparing the same, which can control the morphology of a functional film layer.
[0005] On the one hand, an embodiment of the present application provides an evaporation device, including a reaction chamber, a regulating gas generator, and a crucible and a substrate placement table arranged in the reaction chamber. The crucible and the substrate placement table are arranged relative to each other, and the gas inlet of the regulating gas generator is connected to the reaction chamber. The regulating gas generated by the regulating gas generator enters the reaction chamber and interacts with the transmission gas generated by the crucible to be deposited on the substrate to form a functional film layer.
[0006] As an practicable method, the evaporation device also includes a controller and a pressure detector and a flow controller respectively connected to the controller. The pressure detector is arranged in the reaction chamber and is used to detect the partial pressure of the regulating gas in the reaction chamber. The flow controller is connected to the regulating gas generator. The controller obtains the partial pressure of the regulating gas in the reaction chamber and adjusts the flow controller according to the partial pressure of the regulating gas so that the partial pressure of the regulating gas in the reaction chamber is a preset value.
[0007] As an practicable manner, the regulating gas generator is a water vapor generator, which generates water vapor. The water vapor enters the reaction chamber as the regulating gas and interacts with the transport gas to be deposited on the substrate.
[0008] As an practicable manner, the functional film layer material is a fullerene material.
[0009] As an practicable method, the water vapor partial pressure value is adjusted so that the surface of the functional film layer is in a layered growth mode.
[0010] As an practicable manner, the evaporation device further includes a plating rate controller connected to the crucible, and the plating rate controller controls the plating rate so that the plating rate of the functional film layer is within between.
[0011] As an practicable method, the water vapor partial pressure is adjusted so that the surface of the functional film layer grows in an island-like manner.
[0012] As an practicable manner, the evaporation device further includes a plating rate controller connected to the crucible, and the plating rate controller controls the plating rate so that the plating rate of the functional film layer is within between.
[0013] On the other hand, an embodiment of the present application further provides a method for preparing a solar cell, comprising: providing a substrate; placing the substrate on a substrate placement table of the above-mentioned evaporation device, and depositing a functional film layer on the substrate as a charge transfer layer.
[0014] In another aspect, the embodiments of the present application provide a solar cell, which is prepared by the above-mentioned method for preparing a solar cell and includes a charge transport layer, wherein the material of the charge transport layer is a fullerene material.
[0015] The beneficial effects of the embodiments of the present application include:
[0016] The evaporation device provided by the present application includes a reaction chamber, a regulating gas generator, and a crucible and a substrate placement table arranged in the reaction chamber. The crucible and the substrate placement table are arranged relatively, and the gas delivery port of the regulating gas generator is connected to the reaction chamber. The regulating gas generated by the regulating gas generator enters the reaction chamber and interacts with the transmission gas generated by the crucible to be deposited on the substrate to form a functional film layer. In the process of interaction and deposition of the transmission gas and the regulating gas on the substrate, when the content of the regulating gas is less and the transmission gas is very much in the reaction chamber, the tension between the transmission gas molecules and the substrate is large, and it is easy to form a functional film layer with a layered growth mode on the surface; when the content of the regulating gas is more, the collision probability between the transmission gas molecules and the regulating gas molecules increases, so that the transmission gas molecules can carry the regulating gas molecules to be deposited on the substrate, because the addition of the regulating gas molecules causes the stress between the electron transport layer and the substrate formed by the deposition to change, and the tension between the transmission gas molecules becomes larger. At this time, it is easy to form a functional film layer with an island growth mode on the surface. Therefore, the embodiment of the present application can adjust the morphology of the functional film layer by adjusting the content of the gas in the reaction chamber. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1 One of the structural schematic diagrams of a vapor deposition device provided in an embodiment of the present application;
[0019] Figure 2 A second structural schematic diagram of a vapor deposition device provided in an embodiment of the present application;
[0020] Figure 3 This is a morphology diagram of the electron transport layer of Example 1 of the present application;
[0021] Figure 4 This is a morphology diagram of the electron transport layer of Example 2 of the present application;
[0022] Figure 5 This is a comparison diagram of the open circuit voltages of Example 1 and Example 2 of the present application;
[0023] Figure 6 This is a comparison diagram of short-circuit currents of Example 1 and Example 2 of the present application;
[0024] Figure 7 A schematic diagram of the structure of a solar cell provided in an embodiment of the present application.
[0025] Icons: 100-evaporation device; 110-reaction chamber; 120-regulating gas generator; 130-crucible; 140-substrate placement table; 150-controller; 160-voltage detector; 170-flow controller; 200-solar cell; 210-transparent conductive glass; 220-electron transport layer; 230-perovskite layer; 240-hole transport layer; 250-blocking layer; 260-electrode. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. The components of the embodiments of the present application described and shown in the drawings here can be arranged and designed in various different configurations.
[0027] Therefore, the following detailed description of the embodiments of the present application provided in the accompanying drawings is not intended to limit the scope of the present application for which protection is sought, but merely represents selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0028] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0029] In the description of this application, it should also be noted that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0030] In recent years, perovskite solar cells have attracted much attention due to their high photoelectric conversion efficiency. The morphology and photoelectric properties of the perovskite layer determine the photoelectric conversion efficiency of the cell to a certain extent, so they are particularly important.
[0031] The present application embodiment provides a vapor deposition device 100, such as Figure 1 As shown, it includes a reaction chamber 110, a regulating gas generator 120, and a crucible 130 and a substrate placement table 140 arranged in the reaction chamber 110. The crucible 130 and the substrate placement table 140 are arranged opposite to each other, and the gas inlet of the regulating gas generator 120 is connected to the reaction chamber 110. The regulating gas generated by the regulating gas generator 120 enters the reaction chamber 110 and interacts with the transmission gas generated by the crucible 130 to be deposited on the substrate to form a functional film layer.
[0032] The evaporation device 100 provided in the embodiment of the present application is used to prepare a functional film layer, wherein the functional film layer is used as an electron transport layer, also known as an electron transport layer. Specifically, the evaporation device 100 includes a reaction chamber 110, a crucible 130 and a substrate placement table 140 are arranged in the reaction chamber 110, a coating material is placed in the crucible 130, and the reaction chamber 110 is a vacuum chamber. After the crucible 130 is heated to the sublimation temperature of the coating material, the coating material sublimates to form a transmission gas that diffuses into the reaction chamber 110. At the same time, the adjustment gas generated by the adjustment gas generator 120 enters the reaction chamber 110. A substrate is arranged on the substrate placement table 140. Since the substrate placement table 140 is arranged opposite to the crucible 130 and the substrate placement table 140 is not heated, the temperature of the substrate is relatively low. In this way, when the transmission gas and the adjustment gas in the reaction chamber 110 encounter the substrate, they will be deposited on the substrate. Specifically, the transmission gas and the adjustment gas interact with each other to deposit and grow on the substrate to form an electron transport layer.
[0033] In the process of transport gas and regulating gas being deposited on the substrate, by configuring the ratio of regulating gas and transport gas, the regulating gas and the transport gas produce different reactions, thereby adjusting the ratio of the regulating gas and the transport gas deposited on the substrate, thereby affecting the surface tension of the electron transport layer and the stress between the electron transport layer and the substrate. Specifically, when the content of the regulating gas is less and the transport gas is very much in the reaction chamber 110, the tension between the transport gas molecules and the substrate is large, and it is easy to form an electron transport layer with a layered growth mode on the surface. When the content of the regulating gas is high, the collision probability between the transport gas molecules and the regulating gas molecules increases, so that the transport gas molecules can carry the regulating gas molecules to be deposited on the substrate. Because of the addition of the regulating gas molecules, the stress between the deposited electron transport layer and the substrate changes, and the tension between the transport gas molecules increases. At this time, it is easy to form an electron transport layer with an island growth mode on the surface.
[0034] As can be seen from the above, the embodiment of the present application can adjust the morphology of the charge transport layer by configuring the content of the regulating gas in the reaction chamber 110, thereby adjusting the interface morphology between the electron transport layer and the active layer of the organic electronic device.
[0035] Specifically, the structure of the organic electronic device to which the functional film layer of the embodiment of the present application is applied is not limited, and for example, it can be an organic solar cell, a light emitting diode, or an organic transistor. Specifically, when the organic electronic device is an organic solar cell, the active layer is a perovskite layer as an active layer; when the organic electronic device is a light emitting diode, the active layer is a light emitting layer.
[0036] Optional, such as Figure 2As shown, the evaporation device 100 also includes a controller 150 and a pressure detector 160 and a flow controller 170 respectively connected to the controller 150. The pressure detector 160 is arranged in the reaction chamber 110, and is used to detect the partial pressure of the regulating gas in the reaction chamber 110. The flow controller 170 is connected to the regulating gas generator 120. The controller 150 obtains the partial pressure of the regulating gas in the reaction chamber 110 and adjusts the flow controller 170 according to the partial pressure of the regulating gas, so that the partial pressure of the regulating gas in the reaction chamber 110 is a preset value.
[0037] When the evaporation device 100 evaporates the charge transport layer on the substrate, the controller 150, the pressure detector 160 and the flow controller 170 are set to control the partial pressure of the adjustment gas in the reaction chamber 110 in real time, so that the partial pressure of the adjustment gas is a preset value, which can improve the accuracy of the adjustment and improve the stability of the surface morphology of the electron transport layer 220.
[0038] Specifically, the partial pressure detector 160 detects the reaction chamber 110 in real time and transmits the detected partial pressure value to the controller 150. The controller 150 obtains the partial pressure value and compares it with a threshold value to obtain a regulating signal. The controller 150 controls the flow controller 170 according to the regulating signal to adjust the flow of the regulating gas input into the reaction chamber 110, so that the partial pressure of the regulating gas in the reaction chamber 110 is a preset value.
[0039] The partial pressure value of the regulating gas in the reaction chamber 110 reflects the concentration of the regulating gas in the reaction chamber 110 , and the concentration of the regulating gas can be obtained according to the partial pressure value. The partial pressure value is easier to detect than the concentration.
[0040] like Figure 2 As shown, the pressure detector 160 includes a processing chip and a detection head. In order to avoid malfunction of the processing chip caused by the high temperature of the reaction chamber 110, the detection head can be set in the reaction chamber 110, and the processing chip can be set outside the reaction chamber 110. The detection head is electrically connected to the processing chip. The detection head senses the partial pressure of the regulated gas and transmits the sensed signal to the processing chip. The processing chip processes the processing signal to obtain the pressure value.
[0041] In one achievable manner of the embodiment of the present application, the regulating gas generator 120 is a water vapor generator, which generates water vapor, which enters the reaction chamber 110 as the regulating gas and interacts with the transport gas to be deposited on the substrate. The material of the electron transport layer is fullerene material.
[0042] The water vapor generator vaporizes water to form water vapor. When the regulating gas is water vapor, the electron transport layer is a fullerene material for transmitting electrons. During the evaporation process of the electron transport layer 220, water vapor and fullerene gas coexist in the vacuum chamber. When the content of water vapor is low and there is a lot of fullerene gas in the reaction chamber 110, the tension between the fullerene gas molecules and the substrate is large, and it is easy to form an electron transport layer with a layered growth mode on the surface. When the content of water vapor is high, the collision probability between the fullerene gas molecules and the water vapor molecules increases, so that the fullerene gas molecules can carry water vapor molecules to be deposited on the substrate. Because of the addition of water vapor molecules, the stress between the electron transport layer 220 and the substrate formed by deposition changes, and the tension between the fullerene gas molecules increases. At this time, it is easy to form an electron transport layer with an island growth mode on the surface.
[0043] The material of the electron transport layer is a fullerene material, which is used to transport electrons. Specifically, fullerene includes fullerene and fullerene derivatives. Specifically, fullerene includes at least one of C20, C60, C70, C76, C78, C80 and C84. In addition, the electron transport layer 220 can be a single layer film formed by fullerene or its derivatives, or a multilayer composite film composed of fullerene and fullerene derivatives.
[0044] Those skilled in the art should know that the solar cell 200, as an electronic component, is relatively sensitive to water vapor. In the embodiment of the present application, on the one hand, water vapor is used as a regulating gas and has a relatively low content. On the other hand, water vapor reacts with fullerene gas during the deposition process of the electron transport layer 220. Therefore, the addition of water vapor does not affect the normal operation of the solar cell 200.
[0045] Embodiment 1:
[0046] In one achievable manner of the embodiment of the present application, the water vapor partial pressure value is adjusted so that the surface of the electron transport layer grows in a layered manner.
[0047] Optionally, the evaporation device 100 further includes a plating rate controller 150 connected to the crucible 130, and the plating rate controller 150 controls the plating rate so that the plating rate of the electron transport layer is within between.
[0048] Specifically, after the reaction chamber 110 is evacuated, the pressure in the reaction chamber 110 is less than 1*e -4 Pa, the partial pressure detector 160 is activated, and the water vapor partial pressure in the reaction chamber 110 is made less than 8*e by the flow controller 170. -5 Pa, at this time, the water vapor generator is turned off, the crucible 130 is turned on to heat the crucible 130, and the plating rate of the charge transport layer is controlled by the plating rate controller 150. An electron transport layer 220 is formed on the perovskite layer 230. At this time, fullerene gas molecules are the main gas molecules, and the surface of the formed electron transport layer 220 is a layered growth mode, and the formed surface is relatively flat, wherein the thickness of the electron transport layer 220 is between 8nm and 30nm.
[0049] For example, the organic optical device is a solar cell. When the surface of the electron transport layer 220 is in a layered growth mode, the interface between the charge transport layer and the perovskite layer 230 is uniformly covered and the interface is relatively flat. Figure 3 As shown, this is beneficial to improving the extraction of electron-hole pairs from the perovskite layer 230 and increasing the short-circuit current.
[0050] The specific value of the water vapor partial pressure is not limited in the present embodiment, and can be 7*e -5 Pa, 5*e -5 Pa, 3*e - 5 Pa, preferably, the water vapor partial pressure is less than 5*e -5 Pa.
[0051] The crucible 130 includes a crucible body and a heating assembly, and the plating rate controller 150 is connected to the heating assembly to control the evaporation rate of the transport material by controlling the heating speed of the heating assembly, thereby controlling the plating rate of the charge transport layer.
[0052] Embodiment 2:
[0053] In one achievable manner of the embodiment of the present application, the water vapor partial pressure value is adjusted so that the surface of the functional film layer grows in an island-like manner.
[0054] Optionally, the evaporation device 100 further includes a plating rate controller 150 connected to the crucible 130, and the plating rate controller 150 controls the plating rate so that the plating rate of the electron transport layer is within between.
[0055] Specifically, after the reaction chamber 110 is evacuated, the pressure in the reaction chamber 110 is less than 1*e -4 Pa, the partial pressure detector 160 is activated, and the water vapor partial pressure in the reaction chamber 110 is set to 1*e through the flow controller 170. -3 -5*e -3 Pa, at this time, the water vapor generator is turned off, the crucible 130 is turned on to heat the crucible 130, and the plating rate of the electron transport layer is controlled by the plating rate controller 150. In a vacuum environment, fullerene gas molecules and water vapor molecules are in a state of mass competition, which makes it easy to obtain a thin film state with high surface energy, so that the surface of the electron transport layer grows in an island-like manner.
[0056] When the surface of the electron transport layer 220 is in an island-like growth mode, the contact between the electron transport layer 220 and the perovskite layer 230 is point contact, such as Figure 4 As shown, the extraction of electrons is achieved through point contact, which can reduce the contact ratio between the electron transport layer 220 and the perovskite layer 230, thereby reducing interface non-radiative recombination and increasing the open circuit voltage.
[0057] In order to further verify the beneficial effects of the embodiments of the present application, the open circuit voltage and short circuit current of the solar cells of multiple embodiments 1 and multiple embodiments 2 are measured, and the open circuit voltage and short circuit current of embodiment 1 and embodiment 2 are compared using a scatter plot, as shown in FIG. Figure 5 and Figure 6 As shown, Figure 5 is the open circuit voltage scatter plot, Figure 5 It can be seen that the solar cell with an electron transport layer having an island-like growth pattern on the surface of the second embodiment has a larger open circuit voltage, and the solar cell with an electron transport layer having a layer-like growth pattern on the surface of the first embodiment has a smaller open circuit voltage; Figure 6 is the short-circuit current scatter diagram, Figure 6 It can be seen that the solar cell with the electron transport layer having a layered growth pattern on the surface of the first embodiment has a larger short-circuit current, and the solar cell with the electron transport layer having an island growth pattern on the surface of the second embodiment has a smaller short-circuit current.
[0058] It can be seen that when preparing the electron transport layer 220 of the organic electronic device in the embodiment of the present application, the surface tension between the film-forming molecules and the stress level between the film and the substrate are adjusted by controlling the water vapor partial pressure value in the reaction chamber 110, and the nucleation density is adjusted to adjust the morphology of the electron transport layer 220, thereby adjusting the interface morphology between the electron transport layer and the active layer of the organic electronic device.
[0059] It should be noted that the interface morphology in the first and second embodiments is an exemplary embodiment. On this basis, those skilled in the art can adjust the surface morphology of the electron transport layer 220 by adjusting the water vapor partial pressure and the plating rate of the reaction chamber 110. For example, the surface morphology can also be a mixed morphology, for example, it can be a morphology other than layered and island-shaped, or a mixed morphology. Those skilled in the art can specifically set the water vapor partial pressure and the plating rate of the reaction chamber 110 according to actual conditions.
[0060] Embodiment three:
[0061] On the other hand, the embodiment of the present application further provides a method for preparing a solar cell 200, comprising:
[0062] providing a substrate;
[0063] The substrate is placed on the substrate placement platform 140 of the above-mentioned evaporation device 100, and a functional film layer is deposited on the substrate as an electron transport layer, wherein the electron transport layer is a fullerene material and the surface of the electron transport layer is a layered growth method or an island growth method.
[0064] When the electron transport layer 220 is deposited on the substrate, the water vapor partial pressure and the plating rate in the reaction chamber 110 may be adjusted to adjust the morphology of the electron transport layer 220 , thereby adjusting the performance of the solar cell 200 .
[0065] Embodiment 4:
[0066] In another aspect, the present invention provides a solar cell 200, which is prepared by the above-mentioned method for preparing the solar cell 200. Figure 7 As shown, it includes a charge transport layer, the charge transport layer is a fullerene material, and the surface of the charge transport layer is a layered growth method or an island growth method.
[0067] Specifically, Figure 7 As shown, the solar cell 200 includes a transparent conductive glass 210 and an electron transport layer 220, a perovskite layer 230, a hole transport layer 240, a barrier layer 250 and an electrode 260 sequentially arranged on the transparent conductive glass 210, wherein the perovskite layer 230, as a layer for absorbing photons to generate electron-hole pairs, has the advantages of a wider spectral response and a higher carrier mobility, and can improve the photoelectric conversion efficiency of the solar cell 200. The electron transport layer 220 and the hole transport layer 240, as charge transport layers, are respectively arranged on both sides of the perovskite layer 230, the electron transport layer 220 is used to transport electrons of the electron-hole pairs, and the hole transport layer 240 is used to transport holes in the electron-hole pairs, that is, after the electron-hole pairs generated in the perovskite layer 230 are separated, they are respectively transmitted from both sides to the outside of the solar cell 200 to form the output of electric energy.
[0068] The electron transport layer 220 is used to transport electrons, and the surface of the electron transport layer is a layered growth method or an island growth method.
[0069] The fullerene includes fullerene and fullerene derivatives. Specifically, the fullerene includes at least one of C20, C60, C70, C76, C78, C80 and C84. In addition, the electron transport layer 220 can be a single layer film formed by fullerene or its derivatives, or a multilayer composite film composed of fullerene and fullerene derivatives.
[0070] As a layer that blocks the holes from continuing to move, the blocking layer 250 has a deeper HOMO energy level, can effectively block holes, and is helpful to improve the photoelectric conversion efficiency of the solar cell 200. When the material of the blocking layer 250 is BCP, BCP can be regarded as an electron-rich group because it contains N atoms with lone pairs of electrons in its molecules, which can passivate the halogen vacancy defects on the surface of the perovskite layer 230, play a role in reducing interface recombination and improving charge transfer at the interface; the hydrophobic benzene ring in the BCP molecule is also conducive to enhancing the resistance of the interface to the external environment and improving the stability of the solar cell 200.
[0071] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A vapor deposition device, characterized in that: The invention comprises a reaction chamber, a regulating gas generator, and a crucible and a substrate placing table arranged in the reaction chamber. The crucible and the substrate placing table are arranged opposite to each other. The gas inlet of the regulating gas generator is connected with the reaction chamber. The regulating gas generated by the regulating gas generator enters the reaction chamber and interacts with the transmission gas generated by the crucible to be deposited on the substrate to form a functional film layer.
2. The evaporation device according to claim 1, characterized in that: It also includes a controller and a pressure detector and a flow controller respectively connected to the controller. The pressure detector is arranged in the reaction chamber and is used to detect the partial pressure of the regulating gas in the reaction chamber. The flow controller is connected to the regulating gas generator. The controller obtains the partial pressure of the regulating gas in the reaction chamber and adjusts the flow controller according to the partial pressure of the regulating gas so that the partial pressure of the regulating gas in the reaction chamber is a preset value.
3. The evaporation device according to claim 1, characterized in that: The regulating gas generator is a water vapor generator, which generates water vapor. The water vapor enters the reaction chamber as a regulating gas and interacts with the transmission gas to be deposited on the substrate.
4. The evaporation device according to claim 1, characterized in that: The material of the functional film layer is fullerene material.
5. The evaporation device according to claim 3, characterized in that: The water vapor partial pressure value is adjusted so that the surface of the functional film layer is in a layered growth mode.
6. The evaporation device according to claim 1, characterized in that: The invention also includes a plating rate controller connected to the crucible, wherein the plating rate controller controls the plating rate so that the plating rate of the functional film layer is within a range of between.
7. The evaporation device according to claim 3, characterized in that: The water vapor partial pressure value is adjusted so that the surface of the functional film layer grows in an island shape.
8. The evaporation device according to claim 1, characterized in that: The invention also includes a plating rate controller connected to the crucible, wherein the plating rate controller controls the plating rate so that the plating rate of the functional film layer is within a range of between.
9. A method for preparing a solar cell, characterized in that: include: providing a substrate; The substrate is placed on a substrate placement table of the evaporation device according to any one of claims 1 to 8, and a functional film layer is deposited on the substrate as a charge transport layer.
10. A solar cell, characterized in that: The solar cell is prepared by the method for preparing the solar cell according to claim 9, and comprises a charge transport layer, wherein the material of the charge transport layer is a fullerene material.