High-entropy alloy catalytic electrode plate as well as preparation method and application thereof
Through the preparation method of high-entropy alloy catalytic electrode plates, using mechanical ball milling and laser cladding technology, the problem of scarcity of precious metal catalysts and powder film material peeling is solved, and low-cost, high-activity and stable electrolysis catalytic performance is achieved, which is suitable for large-scale applications. large-scale industrial production.
Patent Information
- Application Number
- CN202410752583.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-25
AI Technical Summary
In existing water electrolysis technology, precious metal catalysts limit large-scale industrial production due to scarcity and high cost, and biological physical peeling is prone to occur between the powder membrane material and the electrode, affecting current density and stability.
Using the preparation method of high-entropy alloy catalytic electrode plates, a low-cost, high-activity and stable catalytic electrode plate is prepared through mechanical ball milling and laser cladding technology, using Fe, Co, Ni, Mo, Ti and other metal powders, combined with Polyethylene binder and zirconia beads are mechanically ball milled and laser treated to form a uniform multi-metal oxide surface structure.
It achieves low-cost, high current density and high-stability electrolysis catalytic performance in an industrial environment, reduces material costs, meets the demand for high-performance electrolysis of water for hydrogen evolution, and provides a cheap and efficient catalyst solution.
Smart Images

Figure CN118835263A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new energy materials, and specifically relates to a high entropy alloy catalytic electrode plate and a preparation method thereof, and an application in the field of electrolytic catalysis. Background Art
[0002] Hydrogen energy has a high intrinsic energy density and H2 combustion can achieve zero CO2 emissions, making it an ideal substitute for fossil fuels. Among the methods of hydrogen production such as biohydrogen production, industrial byproduct hydrogen production, and photocatalytic hydrogen production, electrocatalytic water splitting stands out due to its environmental friendliness and ability to produce high-purity hydrogen. However, the development of water electrolysis technology is hampered by the slow kinetics of the oxygen evolution reaction. Currently, precious metals such as platinum, ruthenium, and palladium are the best catalysts due to their low overpotential. However, precious metals are scarce in nature and are quite expensive, which hinders large-scale industrial production.
[0003] Vigorously develop low-cost, high-activity (500mA / cm 2 Non-precious metal oxygen evolution catalysts with an overpotential as low as 200 mV and excellent stability (activity decay of less than 1% in 1000 hours) are the key to promoting the development of water electrolysis technology. Summary of the invention
[0004] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the main purpose of the present invention is to provide a high entropy alloy catalytic electrode plate, which aims to solve the problem of physical peeling between the powder film material and the electrode under excessive current density. The present invention also provides a preparation method of the high entropy alloy catalytic electrode plate and its application in electrolysis of water.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] In a first aspect, a method for preparing a high entropy alloy catalytic electrode plate comprises the following steps:
[0007] 1) Weighing a prescribed amount of metal powder, and then mechanically ball milling and mixing to prepare alloy powder;
[0008] 2) taking a formulated amount of alloy powder and mixing it with a binder, spreading it on a substrate, and performing a drying process to obtain an intermediate product;
[0009] 3) The intermediate product of step 2) is subjected to laser treatment to prepare a high entropy alloy catalytic electrode plate.
[0010] In some specific embodiments, the metal powder is one of Fe, Co, Ni, Mo, W, Ti or Al, and its molar percentage is Fe: 15% to 20%, Co: 15% to 20%, Ni: 15% to 20%, Mo: 15% to 20%, any one of W, Ti or Al: 15% to 20%; wherein the sum of the atomic percentages of any one of Fe, Co, Ni, Mo, W, Ti or Al is 100%.
[0011] In certain specific embodiments, the conditions for the mechanical ball milling are: at room temperature, the ball-to-material ratio of the mechanical ball milling is 3:1 or 2:1, and the ball milling time is 6-8 hours.
[0012] Furthermore, the ball material is one or more of 95% zirconium oxide beads, agate balls, and aluminum oxide beads, and the diameter of the ball material is 3mm, 4mm, 5mm, 6mm, 8mm and 10mm; during ball milling, the roller speed is 300r / min.
[0013] In some specific embodiments, the mass ratio of the alloy powder to the binder is 4:1, and the binder is a polyvinyl ketone solution with a mass concentration of 1 g / 24 ml.
[0014] In certain specific embodiments, the process parameters of the paving in step 2) are: the thickness of the powder layer is 0.6-2 mm; the process parameters of the drying treatment are treatment at 60-80° C. for 5-6 hours.
[0015] In certain specific embodiments, the process parameters of the laser treatment in step 3) are: laser treatment of the surface coating of the catalytic electrode plate is performed at a laser power of 1000-3000 W and a scanning speed of 240-900 mm / min.
[0016] In some specific embodiments, the particle size of the metal powder in step 1) is 100-500 mesh.
[0017] In a second aspect, a high entropy alloy catalytic electrode plate is obtained by the aforementioned preparation method.
[0018] The third aspect is an application of the aforementioned high entropy alloy catalytic electrode plate in the field of electrolytic catalysis.
[0019] Compared with the prior art, the present invention has at least the following advantages:
[0020] 1) The high entropy alloy catalytic electrode plate provided by the present invention is mainly suitable for electrolytic catalysis in industrial environments (50-80°C, 20-30wt% KOH concentrated alkali solution); the high entropy alloy catalytic electrode plate is made by laser cladding technology; at the same time, a specific element combination is conducive to promoting the cladding layer to transform into a material with higher activity oxides during the OER electrocatalytic reaction. Laser cladding first ensures uniform formation of multi-metal species, and the OER activation reaction promotes the transformation of multi-metals into oxides (surface oxidation reconstruction), realizing unique electrochemical surface reconstruction optimization, thereby realizing the industrial-grade high current activity of the catalytic electrode plate;
[0021] 2) The preparation method provided by the present invention does not use precious metals, but mainly uses iron, cobalt, nickel, molybdenum, and tungsten, aluminum, titanium, chromium, copper and other elements, and the material cost is low. At the same time, the laser cladding process is mature and the manufacturing cost is also low. The prepared high-entropy alloy catalytic electrode has excellent activity and stability. The preparation method is simple, low-cost, and meets the conditions for large-scale preparation. It is of great significance to develop cheap and efficient catalysts suitable for the needs of high-performance water electrolysis and hydrogen evolution. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments or the description of the prior art will be briefly introduced below.
[0023] Figure 1 This is a physical picture of the high entropy alloy catalytic electrode plate in Example 9 of the present invention;
[0024] Figure 2 This is a scanning electron microscope image of the high entropy alloy catalytic electrode plate in Example 9 of the present invention;
[0025] Figure 3 The scanning electron microscope image of the high entropy alloy mixed powder in Example 9 of the present invention is
[0026] Figure 4 is the XRD spectrum of the high entropy alloy catalytic electrode plate in Example 9 of the present invention;
[0027] Figure 5 This is a scanning linear voltammetric curve diagram of the high entropy alloy catalytic electrode plate (P treatment) in Example 9 of the present invention;
[0028] Figure 6 This is a linear voltammetric curve of the high entropy alloy catalytic electrode plate in Example 9 of the present invention after 1000 CV scans. DETAILED DESCRIPTION
[0029] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.
[0030] When a certain amount, concentration or other value or parameter is expressed in the form of a range, a preferred range, or a preferred upper and lower numerical limit, it should be understood that it is equivalent to specifically revealing any range by combining any pair of upper range limits or preferred numerical values with any lower range limit or preferred numerical value, regardless of whether the range is specifically disclosed. Unless otherwise indicated, the numerical range values listed herein include the endpoints of the range, and all integers and fractions within the range.
[0031] Unless otherwise indicated, all percentages, parts, ratios, etc. herein are by weight.
[0032] The materials, methods, and examples herein are illustrative and are not to be construed as limiting unless specifically stated.
[0033] In the following embodiments, the polyvinyl ketone used was purchased from Tianjin Huasheng Chemical Reagent Co., Ltd.; the ball material used was one or more of 95% zirconium oxide beads, agate balls, and aluminum oxide beads, and the diameters of the ball materials were 3mm, 4mm, 5mm, 6mm, 8mm and 10mm, and the mass ratio of 3mm, 4mm, 5mm, 6mm, 8mm and 10mm was 25:33:42:50:66:83; the particle size of the metal powder used was 100-500 mesh.
[0034] The test methods used in the following embodiments include:
[0035] In the following examples, the oxygen evolution performance of the high entropy alloy catalytic electrode plate for water electrolysis was evaluated by scanning the linear voltammetric curve using the CHI760E equipment of Shanghai Chenhua Instrument Co., Ltd.:
[0036] Example 1
[0037] This embodiment provides a method for preparing a high entropy alloy catalytic electrode plate, which comprises the following steps:
[0038] 1) Weigh iron powder, cobalt powder, nickel powder and molybdenum powder in a molar ratio of 1:1:1:1 to prepare 100 g of mixed metal powder, put it into a bottle, and mix it with 300 g of zirconium oxide beads; at room temperature, use a roller mill for mechanical ball milling for 6 h, set the speed to 300 r / min, and mix thoroughly to obtain a front-end product alloy powder;
[0039] 2) The pure iron substrate (iron content> 99%) was coarsely ground on #80, #150, #200, and #400 sandpaper, and then cleaned with alcohol to remove surface oil and make the sample surface flat and smooth; 1g of polyvinyl alcohol and 24ml of deionized water were weighed to prepare a solution to obtain an adhesive;
[0040] 3) The alloy powder and the binder are uniformly mixed in a mass ratio of 4:1, and evenly spread on a pure iron substrate with a coating thickness of 0.6 mm. The mixture is then placed in a drying oven and dried at 70° C. for 5 h to remove surface moisture, thereby obtaining an intermediate product;
[0041] 4) The intermediate product is laser treated with a laser power of 1300 W and a scanning speed of 720 mm / min, the surface coating is clad, and the laser treated sample is wire cut with a cutting thickness of 1 mm to a high entropy alloy catalytic electrode plate.
[0042] Example 2
[0043] This embodiment provides a method for preparing a high entropy alloy catalytic electrode plate, which comprises the following steps:
[0044] 1) Weigh iron powder, cobalt powder, nickel powder and molybdenum powder in a molar ratio of 1:1:1:1 to prepare 100 g of mixed metal powder, put it into a bottle, and mix it with 300 g of zirconium oxide beads; at room temperature, use a roller mill for mechanical ball milling for 6 hours, set the speed to 300 r / min, and mix thoroughly to obtain a front-end product alloy powder;
[0045] 2) A pure nickel substrate (nickel content> 99%) was coarsely ground on #80, #150, #200, and #400 sandpaper, and then cleaned with alcohol to remove surface oil and make the sample surface flat and smooth; 1 g of polyvinyl alcohol and 24 ml of deionized water were weighed to prepare a solution to obtain an adhesive;
[0046] 3) uniformly mixing the alloy powder and the binder in a mass ratio of 4:1, evenly spreading the mixture on a pure iron substrate with a coating thickness of 0.6 mm, and then placing the mixture in a drying oven at 70° C. for 5 h to remove surface moisture, thereby obtaining an intermediate product;
[0047] 4) The intermediate product is laser treated with a laser power of 1300 W and a scanning speed of 720 mm / min, the surface coating is melt-clad, and the sample after laser treatment is wire-cut with a cutting thickness of 1 mm to obtain a high entropy alloy catalytic electrode plate.
[0048] Example 3
[0049] This embodiment provides a method for preparing a high entropy alloy catalytic electrode plate, which comprises the following steps:
[0050] 1) Weigh iron powder, cobalt powder, nickel powder, molybdenum powder and titanium powder in a molar ratio of 1:1:1:1:1 to prepare 100 g of mixed metal powder, put it into a bottle, and mix it with 300 g of zirconium oxide beads; at room temperature, use a roller mill for mechanical ball milling for 6 h, set the speed to 300 r / min, and mix thoroughly to obtain a front-end product alloy powder;
[0051] 2) The pure iron substrate (iron content> 99%) was coarsely ground on #80, #150, #200, and #400 sandpaper, and then cleaned with alcohol to remove surface oil and make the sample surface flat and smooth; 1g of polyvinyl alcohol and 24ml of deionized water were weighed to prepare a solution to obtain an adhesive;
[0052] 3) uniformly mixing the alloy powder and the binder in a mass ratio of 4:1, evenly spreading the mixture on a pure iron substrate with a coating thickness of 0.6 mm, and then placing the mixture in a drying oven at 70° C. for 5 h to remove surface moisture, thereby obtaining an intermediate product;
[0053] 4) The intermediate product is laser treated with a laser power of 1300 W and a scanning speed of 720 mm / min, the surface coating is melt-clad, and the sample after laser treatment is wire-cut with a cutting thickness of 1 mm to obtain a high entropy alloy catalytic electrode plate.
[0054] Example 4
[0055] This embodiment provides a method for preparing a high entropy alloy catalytic electrode plate, which comprises the following steps:
[0056] 1) Weigh iron powder, cobalt powder, nickel powder, molybdenum powder and titanium powder in a molar ratio of 1:1:1:1:1 to prepare 100 g of mixed metal powder, put it into a bottle, and mix it with 300 g of zirconium oxide beads; at room temperature, use a roller mill for mechanical ball milling for 6 h, set the speed to 300 r / min, and mix thoroughly to obtain a front-end product alloy powder;
[0057] 2) A pure nickel substrate (nickel content> 99%) was coarsely ground on #80, #150, #200, and #400 sandpaper, and then cleaned with alcohol to remove surface oil and make the sample surface flat and smooth; 1 g of polyvinyl alcohol and 24 ml of deionized water were weighed to prepare a solution to obtain an adhesive;
[0058] 3) uniformly mixing the alloy powder and the binder in a mass ratio of 4:1, evenly spreading the mixture on a pure iron substrate with a coating thickness of 0.6 mm, and then placing the mixture in a drying oven at a temperature of 60-80° C. for 5 h to remove surface moisture, thereby obtaining an intermediate product;
[0059] 4) The intermediate product is laser treated with a laser power of 1300 W and a scanning speed of 720 mm / min, the surface coating is melt-clad, and the sample after laser treatment is wire-cut with a cutting thickness of 1 mm to obtain a high entropy alloy catalytic electrode plate.
[0060] Example 5
[0061] This embodiment provides a method for preparing a high entropy alloy catalytic electrode plate, which comprises the following steps:
[0062] 1) Weighing iron powder, cobalt powder, nickel powder, molybdenum powder and aluminum powder in a molar ratio of 1:1:1:1:1 to prepare 100 g of mixed metal powder, and mixing with 300 g of zirconium oxide beads; performing mechanical ball milling for 6 h using a roller mill at room temperature, with the speed set to 300 r / min, and mixing thoroughly to obtain a front-end product alloy powder;
[0063] 2) The pure iron substrate (iron content> 99%) was coarsely ground on #80, #150, #200, and #400 sandpaper, and then cleaned with alcohol to remove surface oil and make the sample surface flat and smooth; 1g of polyvinyl alcohol and 24ml of deionized water were weighed to prepare a solution to obtain an adhesive;
[0064] 3) uniformly mixing the alloy powder and the binder in a mass ratio of 4:1, evenly spreading the mixture on a pure iron substrate with a coating thickness of 0.6 mm, and then placing the mixture in a drying oven at 60° C. for 5 h to remove surface moisture, thereby obtaining an intermediate product;
[0065] 4) The intermediate product is laser treated with a laser power of 1300 W and a scanning speed of 720 mm / min, the surface coating is melt-clad, and the sample after laser treatment is wire-cut with a cutting thickness of 1 mm to obtain a high entropy alloy catalytic electrode plate.
[0066] Example 6
[0067] This embodiment provides a method for preparing a high entropy alloy catalytic electrode plate, which comprises the following steps:
[0068] 1) Weigh iron powder, cobalt powder, nickel powder, molybdenum powder and tungsten powder in a molar ratio of 1:1:1:1:1 to prepare 100 g of mixed metal powder, put it into a bottle, and mix it with 300 g of zirconium oxide beads; at room temperature, use a roller mill for mechanical ball milling for 6 h, set the speed to 300 r / min, and mix thoroughly to obtain a front-end product alloy powder;
[0069] 2) The pure iron substrate (iron content> 99%) was coarsely ground on #80, #150, #200, and #400 sandpaper, and then cleaned with alcohol to remove surface oil and make the sample surface flat and smooth; 1g of polyvinyl alcohol and 24ml of deionized water were weighed to prepare a solution to obtain an adhesive;
[0070] 3) uniformly mixing the alloy powder and the binder in a mass ratio of 4:1, evenly spreading the mixture on a pure iron substrate with a coating thickness of 0.6 mm, and then placing the mixture in a drying oven at 70° C. for 5 h to remove surface moisture, thereby obtaining an intermediate product;
[0071] 4) The intermediate product is laser treated with a laser power of 1500 W and a scanning speed of 720 mm / min, the surface coating is melt-clad, and the sample after laser treatment is wire-cut with a cutting thickness of 1 mm to obtain a high entropy alloy catalytic electrode plate.
[0072] Example 7
[0073] This embodiment provides a method for preparing a high entropy alloy catalytic electrode plate, which comprises the following steps:
[0074] 1) Weigh iron powder, cobalt powder, nickel powder, molybdenum powder and tungsten powder in a molar ratio of 1:1:1:1:1 to prepare 100 g of mixed metal powder, put it into a bottle, and mix it with 300 g of zirconium oxide beads; at room temperature, use a roller mill for mechanical ball milling for 6 h, set the speed to 300 r / min, and mix thoroughly to obtain a front-end product alloy powder;
[0075] 2) A pure nickel substrate (nickel content> 99%) was coarsely ground on #80, #150, #200, and #400 sandpaper, and then cleaned with alcohol to remove surface oil and make the sample surface flat and smooth; 1 g of polyvinyl alcohol and 24 ml of deionized water were weighed to prepare a solution to obtain an adhesive;
[0076] 3) uniformly mixing the alloy powder and the binder in a mass ratio of 4:1, evenly spreading the mixture on a pure iron substrate with a coating thickness of 0.6 mm, and then placing the mixture in a drying oven at 70° C. for 5 h to remove surface moisture, thereby obtaining an intermediate product;
[0077] 4) The intermediate product is laser treated with a laser power of 1500 W and a scanning speed of 720 mm / min, the surface coating is melt-clad, and the sample after laser treatment is wire-cut with a cutting thickness of 1 mm to obtain a high entropy alloy catalytic electrode plate.
[0078] Example 8
[0079] This embodiment provides a method for preparing a high entropy alloy catalytic electrode plate, which comprises the following steps:
[0080] 1) Weigh 100 g of mixed metal powder of iron powder, cobalt powder, nickel powder, molybdenum powder and aluminum powder in a molar ratio of 1:1:1:1:0.2, put it into a bottle, and mix it with 300 g of zirconium oxide beads; at room temperature, use a roller mill for mechanical ball milling for 6 h, set the speed to 300 r / min, and mix thoroughly to obtain a front-end product alloy powder;
[0081] 2) The pure iron substrate (iron content> 99%) was coarsely ground on #80, #150, #200, and #400 sandpaper, and then cleaned with alcohol to remove surface oil and make the sample surface flat and smooth; 1g of polyvinyl alcohol and 24ml of deionized water were weighed to prepare a solution to obtain an adhesive;
[0082] 3) uniformly mixing the alloy powder and the binder in a mass ratio of 4:1, evenly spreading the mixture on a pure iron substrate with a coating thickness of 0.6 mm, and then placing the mixture in a drying oven at 70° C. for 5 h to remove surface moisture, thereby obtaining an intermediate product;
[0083] 4) The intermediate product is laser treated with a laser power of 2100 W and a scanning speed of 720 mm / min, the surface coating is melt-clad, and the sample after laser treatment is wire-cut with a cutting thickness of 1 mm to obtain a high entropy alloy catalytic electrode plate.
[0084] Example 9
[0085] This embodiment provides a method for preparing a high entropy alloy catalytic electrode plate, which comprises the following steps:
[0086] 1) Weigh 100 g of mixed metal powder of iron powder, cobalt powder, nickel powder, molybdenum powder and aluminum powder in a molar ratio of 1:1:1:1:0.5, put it into a bottle, and mix it with 300 g of zirconium oxide beads; at room temperature, use a roller mill for mechanical ball milling for 6 h, set the speed to 300 r / min, and mix thoroughly to obtain a front-end product alloy powder;
[0087] 2) The pure iron substrate (iron content> 99%) was coarsely ground on #80, #150, #200, and #400 sandpaper, and then cleaned with alcohol to remove surface oil and make the sample surface flat and smooth; 1g of polyvinyl alcohol and 24ml of deionized water were weighed to prepare a solution to obtain an adhesive;
[0088] 3) uniformly mixing the alloy powder and the binder in a mass ratio of 4:1, evenly spreading the mixture on a pure iron substrate with a coating thickness of 0.6 mm, and then placing the mixture in a drying oven at 70° C. for 5 h to remove surface moisture, thereby obtaining an intermediate product;
[0089] 4) The intermediate product is laser treated with a laser power of 2100 W and a scanning speed of 720 mm / min, the surface coating is melt-clad, and the sample after laser treatment is wire-cut with a cutting thickness of 1 mm to obtain a high entropy alloy catalytic electrode plate.
[0090] Performance Testing:
[0091] The present application also conducts a performance test on the prepared high entropy alloy catalytic electrode plate. Specifically, taking Example 9 as an example, the prepared FeCoNiMoAl 0.5 High entropy alloy performance test:
[0092] 1) Electrical performance test
[0093] This application takes Example 9 as an example, and its electrochemical tests are all performed at room temperature using a CHI760E electrochemical workstation.
[0094] The test sample preparation method of the high entropy alloy catalytic electrode plate is as follows: cut the sample into 1mm thickness (including the coating surface), place it in a beaker, add an appropriate amount of 95% anhydrous ethanol, place the beaker in an ultrasonic cleaner for 5-10min, then take it out and dry it with a hair dryer, and use 1M KOH (pH=14) solution as an alkaline electrolyte for testing. A three-electrode system is used in the test, using a carbon rod as a counter electrode and an Ag / AgCl electrode as a reference electrode. The high entropy alloy catalytic electrode plate is sandwiched between a platinum sheet electrode as a working electrode, and a scanning linear voltammetry curve test is performed, with a scanning speed of 0.1mV / s and a potential range of (-0.8~1.8V). The measured data is calibrated with a reversible hydrogen electrode (RHE) according to the equation:
[0095] E RHE =E Ag / AgCl +1.02V
[0096] Test results such as Figure 5 As shown in the figure, it is found that the catalytic electrode plate only needs an electrolysis voltage of 1.648V to generate 1.5A / cm 2 The OER catalytic activity at a current density of 2.5 is excellent.
[0097] 2) Appearance test
[0098] This application takes Example 9 as an example to test the electrochemical oxygen evolution performance of the intermediate product and the prepared high entropy alloy catalytic electrode plate in the preparation method of this application;
[0099] The results are as follows Figure 1 , 2 , 3, 4 and 5, from Figure 1It can be seen that the high entropy alloy electrode plate is silvery-white with gullies after laser cladding, and there is no obvious crack on the cladding surface. The coating after grinding has no obvious pore defects. From the appearance, the forming quality is good. After grinding, it is a smooth silvery-white coating (the coating thickness is about 0.5 mm). Figure 2 It can be seen that the microstructure of the high entropy alloy coating has fine and uniform grains. Figure 3 It can be seen that the powder is nearly spherical as a whole, with an average particle size of about 150μm, mainly distributed in the range of 70μm-150μm, and the elements of the alloy powder are evenly distributed without obvious segregation. Figure 4 It can be seen that the high-entropy alloy coating is a uniform face-centered cubic solid solution structure. Since the Al element has a larger atomic radius than other elements, after adding the Al element, Al occupies more positions and the material may undergo lattice distortion, making the electrochemical active area larger and providing more active sites. In summary, the high-entropy alloy catalytic electrode plate has excellent performance.
[0100] 3) Stability test
[0101] Test method: Stability test of catalytic electrode plate: within the voltage window of polarization curve, continuously scan 1000 or even 10000 CVs, and then check the overlap of the two LSVs before and after CV, which mainly characterizes the redox performance of catalytic electrode plate and whether it is stable after redox.
[0102] The test results are as follows Figure 6 As shown in the figure, it can be seen that the LSV curves of the high entropy alloy electrode plate after 10,000 CV cycles are basically coincident, and the high entropy alloy electrode plate has excellent stability.
[0103] The preparation method of the high entropy alloy catalytic electrode plate provided in the present application is to select one of the cheap metal powders of Fe, Co, Ni, Ti, or Mo, W, Al, and perform laser treatment at room temperature, so that the prepared high entropy alloy catalytic electrode has excellent activity and stability; this method can provide a new idea and method for synthesizing efficient and stable catalytic materials.
[0104] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.
Claims
1. A method for preparing a high entropy alloy catalytic electrode plate, characterized in that: The steps include: 1) Weighing a prescribed amount of metal powder, and then mechanically ball milling and mixing to prepare alloy powder; 2) taking a formulated amount of alloy powder and mixing it with a binder, spreading it on a substrate, and performing a drying process to obtain an intermediate product; 3) The intermediate product of step 2) is subjected to laser treatment to prepare a high entropy alloy catalytic electrode plate.
2. The method for preparing a high entropy alloy catalytic electrode plate according to claim 1, characterized in that: The metal powder is one of Fe, Co, Ni, Mo, W, Ti, and Al, and its atomic percentage is Fe: 15% to 20%, Co: 15% to 20%, Ni: 15% to 20%, Mo: 15% to 20%, and any one of W, Ti or Al: 15% to 20%; wherein the sum of the atomic percentages of any one of Fe, Co, Ni, Mo, W, Ti, and Al is 100%.
3. The method for preparing a high entropy alloy catalytic electrode plate according to claim 1, characterized in that: The conditions of the mechanical ball milling are as follows: at room temperature, the ball-to-material ratio of the mechanical ball milling is 3:1 or 2:1, and the ball milling time is 6-8h.
4. The method for preparing a high entropy alloy catalytic electrode plate according to claim 3, characterized in that: The ball material is one or more of 95% zirconium oxide beads, agate balls, and aluminum oxide beads, and the diameter of the ball material is 3mm, 4mm, 5mm, 6mm, 8mm and 10mm; during ball milling, the roller speed is 300r / min.
5. The method for preparing a high entropy alloy catalytic electrode plate according to claim 1, characterized in that: The mass ratio of the alloy powder to the binder is 4:1, and the binder is a polyvinyl ketone solution with a mass concentration of 1 g / 24 ml.
6. The method for preparing a high entropy alloy catalytic electrode plate according to claim 4, characterized in that: The process parameters of the paving in step 2) are: the thickness of the powder layer is 0.6-2 mm; the process parameters of the drying treatment are treatment at 60-80° C. for 5-6 hours.
7. The method for preparing a high entropy alloy catalytic electrode plate according to claim 1, characterized in that: The process parameters of the laser treatment in step 3) are: laser treatment of the surface coating of the catalytic electrode plate is performed at a laser power of 1000-3000 W and a scanning speed of 240-900 mm / min.
8. The method for preparing a high entropy alloy catalytic electrode plate according to claim 4, characterized in that: The step is characterized in that The particle size of the metal powder in step 1) is 100-500 mesh.
9. A high entropy alloy catalytic electrode plate obtained according to the preparation method described in any one of claims 1 to 8.
10. Use of the high entropy alloy catalytic electrode plate according to claim 9 in the field of electrolytic catalysis.
Citation Information
Cited By
High-entropy alloy electrocatalyst with core-shell structure as well as preparation method and application of high-entropy alloy electrocatalyst
CN120400899A