Physical domain infrared visual pattern preparation and implementation method
By printing and spraying complex polymer patterns on active metal or alloy films, and combining with electric spray heads to spray acidic solutions, efficient and low-cost infrared vision patterns are generated, which solves the problems of robustness and infrared vision simulation materials in the existing technology. The cost issue enables the formation and large-area use of complex-shaped images.
Patent Information
- Application Number
- CN202410862759.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-25
AI Technical Summary
The existing physical domain lacks infrared visual simulation materials designed for AI sensitivity, and it is difficult for electrically driven switching infrared feature devices to achieve low cost, low energy consumption or large area use, and it is difficult to form complex-shaped infrared images.
Use a UV printer to print transferable complex polymer patterns and transfer them to active metal or alloy films, combine them with electric spray heads to spray acidic solutions, and use infrared thermal imaging cameras to take pictures to generate specific infrared visual patterns, which can be achieved by adjusting spray parameters Precise control of temperature and concentration.
It achieves large-area infrared vision simulation with high robustness and manufacturability, improves the robustness of visual recognition, reduces the complexity of sample features, and significantly reduces costs and energy consumption.
Smart Images

Figure CN118837166A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of artificial intelligence technology, and in particular to a method for preparing and realizing physical domain infrared vision patterns. Background Art
[0002] In recent years, artificial intelligence (AI) has revolutionized computer vision, demonstrating capabilities far beyond those of humans. This has sparked interest in exploring the vulnerabilities of AI vision systems. To achieve this goal, researchers have proposed a variety of materials and devices in the physical domain, including composite materials that mimic background color, shape, and spectrum, multilayer materials with camouflage properties in multiple wavelengths, dynamic devices that actively control optical and infrared features, and metamaterial devices that can intelligently modulate incident microwaves. These technologies enable simulation, fusion, modulation, and imitation of different features in the physical domain, providing valuable physical examples.
[0003] At present, the physical domain lacks infrared vision simulation materials designed for AI sensitivity, or these materials and devices do not have good physical usage characteristics. For example, combustion can only produce rough point-like infrared images, and it is difficult to form images with complex shapes. And electrically driven infrared characteristic transformation devices (such as variable temperature devices, variable emissivity devices) are difficult to achieve low cost, low energy consumption or large-area use. Therefore, it is urgent to develop new infrared vision simulation materials that are both highly robust and highly manufacturable and have significant physical advantages. Summary of the invention
[0004] Based on this, it is necessary to provide a method for preparing and realizing physical domain infrared visual patterns to address the above technical problems.
[0005] A method for preparing and realizing a physical domain infrared visual pattern based on an ultraviolet printer, the method comprising:
[0006] Print transferable complex polymer patterns using a UV printer.
[0007] Transfer a complex polymer pattern onto one of the surfaces of an active metal or alloy film.
[0008] A polymer film with a predetermined thickness is sprayed on the area without the complex polymer pattern on the surface of the active metal or alloy film attached with the complex polymer pattern by using a polymer spraying tool.
[0009] The acid solution is atomized by an electric spray head and sprayed onto the surface of the active metal or alloy film to which no complex polymer pattern is attached, and an infrared thermal imager is used to take pictures to obtain a specific infrared visual pattern.
[0010] In one embodiment, a UV printer is used to print a transferable complex polymer pattern, including:
[0011] The UV-curable polymer is printed onto the adhesive surface of the polyethylene terephthalate transfer film by a UV printer and cured by ultraviolet light to eventually form a transferable polymer pattern. Different colors of coatings are then printed on the polymer pattern to produce visible light characteristics.
[0012] In one embodiment, transferring a polymer pattern onto one surface of an active metal or alloy film comprises:
[0013] The ethylene terephthalate release film with the adhesive side is peeled off, and then the adhesive side is adhered to the active metal or alloy film; the ethylene terephthalate film on the other side is peeled off, leaving a complex polymer pattern on the active metal or alloy film.
[0014] In one embodiment, an acid solution is atomized by an electric spray head and sprayed onto the surface of the active metal or alloy film to which the polymer pattern is not attached, and an infrared thermal imager is used to take a picture to obtain a specific infrared visual pattern, including:
[0015] The device is used to unfold an active metal or alloy film with a specific polymer pattern and fix the active metal or alloy film on a frame.
[0016] An electric atomizing nozzle is used to atomize the acid solution and spray it onto the surface of the active metal or alloy film where no polymer pattern is attached; at the same time, an infrared thermal imager is used to observe the surface of the active metal or alloy film where the polymer pattern is attached to obtain a specific infrared visual pattern.
[0017] In one embodiment, the method further includes: if it is necessary to prepare an infrared visual pattern larger than the area of a single active metal or alloy film, multiple active metal or alloy films are spliced together and multiple electric atomizing nozzles are deployed to expand the coverage.
[0018] In one embodiment, the acidic solution is dilute hydrochloric acid, dilute sulfuric acid, dilute nitric acid or acetic acid.
[0019] In one of the embodiments, the temperature of the heating process is precisely controlled by adjusting the spraying time of the atomized acid solution, the concentration of the acid solution, or the power and spraying pattern of the electric spray head.
[0020] A method for preparing and realizing a physical domain infrared vision pattern based on a mask, the method comprising:
[0021] Make a mask of the target object.
[0022] The mask plate is laid on one surface of the active metal or alloy film, and the polymer coating is coated on the surface of the active metal or alloy film by scraping or spraying to obtain the active metal or alloy film coated with the polymer pattern.
[0023] A polymer film having a predetermined thickness is sprayed on the area without the polymer pattern on the surface of the active metal or alloy film coated with the polymer coating by using a polymer spraying tool.
[0024] The acid solution is atomized by an electric spray head and sprayed onto the surface of the active metal or alloy film that is not coated with a polymer pattern, and an infrared thermal imager is used to take pictures to obtain a specific infrared visual pattern.
[0025] In one embodiment, the method further includes: if it is necessary to prepare an infrared visual pattern larger than the area of a single active metal or alloy film, multiple active metal or alloy films are spliced together and multiple electric atomizing nozzles are deployed to expand the coverage.
[0026] In one of the embodiments, the temperature of the heating process is precisely controlled by adjusting the spraying time of the atomized acid solution, the concentration of the acid solution, or the power and spraying pattern of the electric spray head.
[0027] The above-mentioned method for preparing and realizing infrared visual patterns in the physical domain includes: using an ultraviolet printer to print a transferable complex polymer pattern; transferring the complex polymer pattern to one of the surfaces of an active metal or alloy film; using a polymer spraying tool to spray a layer of polymer film of a predetermined thickness on the area without a complex polymer pattern on the surface of the active metal or alloy film with the complex polymer pattern attached; using an electric spray head to atomize the acid solution and spray it on the surface of the active metal or alloy film without the complex polymer pattern attached, and taking pictures with an infrared thermal imager to obtain a specific infrared visual pattern. This method generates visual samples using the key features of the object, which can improve the robustness of visual recognition, maintain the high sensitivity (high detection rate) of the visual sample in multiple AI visual models, and significantly reduce the feature complexity of the sample, making it easier to be manufactured and realized in the physical domain. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a flow chart of a method for preparing and realizing a physical domain infrared visual pattern based on an ultraviolet printer in one embodiment;
[0029] Figure 2 The polymer patterns of several different targets in another embodiment; wherein (a) is a person, (b) is a vehicle, (c) is a vehicle, (d) is a person and a vehicle, and (e) is an airplane;
[0030] Figure 3 A specific polymer pattern transferred onto a magnesium foil in another embodiment;
[0031] Figure 4 is a schematic diagram of realizing a specific infrared visual pattern and a diagram of actual effect in another embodiment;
[0032] Figure 5 The figure is a flow chart of a method for preparing and realizing a physical domain infrared vision pattern based on a mask in an embodiment. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0034] Metals exhibit unique infrared properties in the physical domain and are considered to be suitable materials for constructing infrared band visual simulations. For example, through the free electron shielding effect, metals have very low infrared emissivity in the bulk state, which can effectively suppress infrared signals; through the hybridized localized surface plasmon resonance effect, metals exhibit significant high infrared absorption at the nanoscale, which can be used as ideal broadband infrared absorbers; by bridging the nano and macro state properties, the infrared emissivity of metals can be dynamically regulated and the effect of dynamic thermal camouflage can be obtained; through electrical heating or exothermic reactions, metals can quickly release a large amount of heat to produce high-temperature infrared features. In addition, due to the abundance, ductility and machinability of metals, they can be manufactured on a large scale and at low cost, and complex designs and structures can be realized, and finally highly robust infrared visual simulations can be realized in the physical domain. Simulated samples generated using key features of objects can improve the robustness of visual simulations. This method can maintain the high sensitivity (high detection rate) of samples in multiple AI visual models, while significantly reducing the feature complexity of samples, making them easier to manufacture and implement in the physical domain.
[0035] In one embodiment, Figure 1 As shown, a method for preparing and realizing a physical domain infrared visual pattern is provided, and the method comprises the following steps:
[0036] Step 100: Printing a transferable complex polymer pattern using a UV printer.
[0037] Specifically, during the printing process, the UV printer uses a nozzle to spray the UV-curable polymer onto the printing material. While spraying the UV-curable polymer, the UV printer immediately irradiates the sprayed UV-curable polymer with UV light. The UV light can cause the chemical substances in the UV-curable polymer to polymerize, solidify and harden quickly.
[0038] Step 102: Transferring a complex polymer pattern onto one of the surfaces of the active metal or alloy film.
[0039] Specifically, active metal or alloy film refers to a metal or alloy film with high chemical reaction activity, which can be a pure magnesium film, or a magnesium alloy (such as magnesium copper, magnesium lithium, magnesium zinc, etc.), or an active metal or alloy film made of active metal or alloy materials that easily produce exothermic reactions with acidic solutions.
[0040] The thickness of the active metal or alloy film can be customized. The thicker the metal, the more chemical energy it contains and the longer it can generate heat. The thinner it is, the shorter the heating time, but at the same time the active metal or alloy film is more flexible and can be better rolled up for storage and convenient transportation.
[0041] When the active metal or alloy film is magnesium foil, due to the high reactivity of magnesium metal, the response time of the infrared pattern generated by the exothermic reaction is very short, and the preset maximum temperature can be reached in about 2 seconds. When the thickness of the magnesium foil is 3mm, its area heating power density can reach 2.5×10 5 W / m 2 In addition, by further reducing the thickness of the magnesium foil, its heating power can be further improved.
[0042] Taking the active metal or alloy film as magnesium foil for illustration: In order to accurately replicate complex infrared patterns in the physical domain, this embodiment uses ultraviolet digital printing transfer technology to transfer complex polymer patterns on one surface of the magnesium foil. Among them, the polymer material with high emissivity serves as the main pattern part of the infrared simulation, while the magnesium foil with low emissivity serves as the background part. During the heating process, magnesium will suppress thermal radiation, causing its radiation temperature to be close to the ambient temperature, while the polymer will be close to the black body radiation temperature, which can be used to simulate the infrared radiation characteristics of real objects.
[0043] Step 104: using a polymer spraying tool, spray a layer of polymer film of a predetermined thickness on the area without the complex polymer pattern on the surface of the active metal or alloy film to which the complex polymer pattern is attached.
[0044] Specifically, after the polymer pattern is pasted, the emissivity of the bare metal surface without the polymer pattern on the surface of the active metal or alloy film pasted with the complex polymer pattern can be regulated. For example, a polymer spraying tool is used to spray another layer of polymer film of a specific thickness, so as to accurately control the emissivity of the bare metal surface. As the thickness of the sprayed polymer increases, the infrared emissivity of the metal surface can also increase from close to 0 to a specific value.
[0045] It is worth noting that the polymer sprayed and the polymer used to make the complex polymer pattern can be the same or different.
[0046] Step 106: Atomize the acid solution using an electric spray head and spray it onto the surface of the active metal or alloy film where the specific polymer pattern is not attached, and simultaneously take a picture using an infrared thermal imager to obtain a specific infrared visual pattern.
[0047] Specifically, by combining the exothermic reaction between a large area of active metal or alloy film and atomized acid with the high emissivity contrast surface of active metal / polymer, a lightweight, large area, uniform, controllable, extremely fast and cost-effective infrared visual pattern can be developed.
[0048] A single atomizing nozzle can evenly heat an area over 50×50cm 2 And at this size, the temperature difference from the center to the edge of the active metal or alloy film does not exceed 3°C, proving that the exothermic reaction achieved by atomizing the acidic solution has the ability to generate heat evenly over a large area. Therefore, by adding multiple atomizing nozzles, the heat release area can be efficiently expanded, achieving uniform heat release over a larger area and larger size.
[0049] Take magnesium foil as an example for active metal or alloy film: the infrared pattern is mainly composed of magnesium foil, polymer pattern and atomization spray system, which is low-cost. Among them, the cost of metal magnesium accounts for a large proportion. When 1mm thick magnesium foil is used, the material cost is only 32 yuan / m 2 (Calculated based on a magnesium price of RMB 18,950 / ton).
[0050] In the above-mentioned method for preparing and realizing infrared visual patterns in the physical domain, the method includes: using an ultraviolet printer to print a transferable complex polymer pattern; transferring the complex polymer pattern to one of the surfaces of an active metal or alloy film; using a polymer spraying tool to spray a layer of polymer film of a predetermined thickness on the area without a complex polymer pattern on the surface of the active metal or alloy film with the complex polymer pattern attached; using an electric spray head to atomize the acid solution and spray it on the surface of the active metal or alloy film without the complex polymer pattern attached, and using an infrared thermal imager to take pictures to obtain a specific infrared visual pattern. This method generates visual samples using the key features of the object, which can improve the robustness of visual recognition, maintain the high sensitivity (high detection rate) of the visual sample in multiple AI visual models, and significantly reduce the feature complexity of the sample, making it easier to be manufactured and realized in the physical domain.
[0051] In one embodiment, step 100 includes: printing a UV-curable polymer onto the adhesive surface of a polyethylene terephthalate transfer film by a UV printer, and curing it by UV light to finally form a transferable polymer pattern, and then printing different colors of coatings on the polymer pattern to produce visible light characteristics.
[0052] Specifically, first, a UV-curable polymer is printed onto the adhesive surface of a polyethylene terephthalate (PET) transfer film by a commercial UV printer, and then cured by ultraviolet light to finally form a transferable polymer pattern.
[0053] Figure 2 Shown are polymer patterns of several different targets; (a) is a person, (b) is a vehicle, (c) is a vehicle, (d) is a person and a vehicle, and (e) is an airplane.
[0054] In one embodiment, step 102 includes: peeling off the ethylene terephthalate release film with the adhesive side, and then adhering the adhesive side downward to the active metal or alloy film; and then peeling off the ethylene terephthalate film on the other side, leaving a complex polymer pattern on the active metal or alloy film.
[0055] Specifically, first, the PET release film with the adhesive side is torn off, and then the side with the adhesive facing down is adhered to the magnesium foil. The thickness of the magnesium foil can be 0.1mm to 5mm. The thinner the magnesium foil, the better its flexibility and the easier it is to curl and store. Then, the PET film on the other side is peeled off, and finally, a complex polymer pattern is left on the magnesium foil. The polymer pattern transferred to the magnesium foil is as follows: Figure 3 shown.
[0056] In one embodiment, step 104 includes: using a device to unfold an active metal or alloy film with a specific polymer pattern, and fixing the active metal or alloy film on a frame; using an electric atomizing nozzle to atomize and spray the acidic solution onto the surface of the active metal or alloy film where the polymer pattern is not attached; and simultaneously using an infrared thermal imager to observe the surface of the active metal or alloy film where the polymer pattern is attached to obtain a specific infrared visual pattern.
[0057] Specifically, the schematic diagram and actual effect diagram of the infrared visual pattern are as follows: Figure 4 shown.
[0058] The acid solution is sprayed by atomization using an electric atomizing nozzle. The acid solution used can be dilute hydrochloric acid, dilute sulfuric acid, dilute nitric acid or acetic acid, etc. Usually, the material of the atomizing nozzle is a plastic or metal material that is resistant to corrosion by the acid solution. The concentration of the sprayed acid solution is adjusted according to the maximum temperature to be reached. When a higher temperature is required, an acid solution with a higher concentration is used. At the same time, the spray flow rate can also be adjusted. Generally, the flow rate of a single nozzle is controlled between 0.05 and 20 liters / minute, and the spray angle can be adjusted, generally between 10° and 150°. If a larger area needs to be covered for atomization spraying, the spray angle is fixed at the maximum angle. In addition, when performing infrared simulation, the magnesium foil with a specific polymer pattern is first unfolded using a device and fixed to a frame, and then the nozzle is fixed at a distance of 10-200 cm from the back of the magnesium foil for operation. If a larger area of infrared visual pattern preparation is required, multiple pieces of magnesium foil can be spliced and multiple electric atomizing nozzles can be deployed to expand the coverage.
[0059] In one embodiment, the method further includes: if it is necessary to prepare an infrared visual pattern larger than the area of a single active metal or alloy film, multiple active metal or alloy films are spliced together and multiple electric atomizing nozzles are deployed to expand the coverage.
[0060] In one embodiment, the acidic solution is dilute hydrochloric acid, dilute sulfuric acid, dilute nitric acid or acetic acid.
[0061] Specifically, the concentration of the acidic solution can be adjusted. Different concentrations result in different reaction rates, thereby controlling the rate and temperature of heat release.
[0062] In one of the embodiments, the temperature of the heating process is precisely controlled by adjusting the spraying time of the atomized acid solution, the concentration of the acid solution, or the power and spraying pattern of the electric spray head.
[0063] Specifically, by adjusting the spraying time of the atomized acid solution, the concentration of the acid solution, or the power and spraying pattern of the electric spray head, the temperature of the heating process can be precisely controlled. Specifically, the spraying flow rate of the acid solution can be controlled by intermittent spraying, thereby regulating the reaction temperature. The longer the intermittent time of spraying, the lower the rate of the exothermic reaction, the less chemical energy released, and the less infrared radiation generated; in addition, the rate of the exothermic chemical reaction can be controlled by adjusting the concentration of the solution. The lower the concentration, the lower the rate of the exothermic reaction, the less chemical energy released, and the less infrared radiation generated.
[0064] As a preferred active metal or alloy film, magnesium foil is used. When the thickness of the magnesium foil is 3 mm and the concentration of the atomized acid solution is 6 mol / L, the energy density of the magnesium foil during heating is about 5320 Wh / kg and the power density is about 1216.7 kW / kg. This value far exceeds the energy and power density of commercial batteries (energy and power density are 254 Wh / kg and 1.5 kW / kg, respectively) and capacitors (energy and power density are 5 Wh / kg and 20 kW / kg, respectively) during electrical heating.
[0065] It should be understood that although Figure 1 The steps in the flowchart are shown in sequence as indicated by the arrows, but these steps are not necessarily executed in the order indicated by the arrows. Unless otherwise specified in this document, there is no strict order restriction for the execution of these steps, and these steps can be executed in other orders. Moreover, Figure 1 At least part of the steps may include multiple sub-steps or multiple stages. These sub-steps or stages are not necessarily executed at the same time, but can be executed at different times. The execution order of these sub-steps or stages is not necessarily sequential, but can be executed in turn or alternately with other steps or at least part of the sub-steps or stages of other steps.
[0066] In one embodiment, Figure 5 As shown, a method for preparing and realizing a physical domain infrared vision pattern based on a mask is provided, and the method comprises:
[0067] Step 500: Make a mask plate of the target object.
[0068] Step 502: Place a mask plate on one surface of the active metal or alloy film, and apply a polymer coating on the surface of the active metal or alloy film by scraping or spraying to obtain an active metal or alloy film coated with a complex polymer pattern.
[0069] Specifically, patterning can be performed by scraping or spraying another polymer film with customizable thickness onto the surface of the active metal or alloy film, and the emissivity of the exposed metal surface can be adjusted by the thickness of the film, thereby further achieving precise control of the emissivity / infrared characteristics of these areas.
[0070] Step 504: using a polymer spraying tool, spray a polymer film of a predetermined thickness on the area without a polymer pattern on the surface of the active metal or alloy film coated with the polymer coating.
[0071] Step 506: Atomize the acid solution using an electric spray head and spray it onto the surface of the active metal or alloy film that is not coated with the polymer pattern, and simultaneously take a picture using an infrared thermal imager to obtain a specific infrared visual pattern.
[0072] Specifically, the acidic solution is dilute hydrochloric acid, dilute sulfuric acid, dilute nitric acid or acetic acid. The concentration of the acidic solution can be adjusted, and different concentrations result in different reaction rates, thereby controlling the rate and temperature of heat release.
[0073] The temperature of the heating process can be precisely controlled by adjusting the spraying time of the atomized acid solution, the concentration of the acid solution or the power and spraying pattern of the electric spray head.
[0074] In one embodiment, the method further includes: if it is necessary to prepare an infrared visual pattern larger than the area of a single active metal or alloy film, multiple active metal or alloy films are spliced together and multiple electric atomizing nozzles are deployed to expand the coverage.
[0075] In one of the embodiments, the temperature of the heating process is precisely controlled by adjusting the spraying time of the atomized acid solution, the concentration of the acid solution, or the power and spraying pattern of the electric spray head.
[0076] Specifically, by adjusting the spraying time of the atomized acid solution, the concentration of the acid solution, or the power and spraying pattern of the electric spray head, the temperature of the heating process can be precisely controlled. Specifically, the spraying flow rate of the acid solution can be controlled by intermittent spraying, thereby regulating the reaction temperature. The longer the intermittent time of spraying, the lower the rate of the exothermic reaction, the less chemical energy released, and the less infrared radiation generated; in addition, the rate of the exothermic chemical reaction can be controlled by adjusting the concentration of the solution. The lower the concentration, the lower the rate of the exothermic reaction, the less chemical energy released, and the less infrared radiation generated.
[0077] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0078] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
Claims
1. A method for preparing and realizing a physical domain infrared visual pattern based on an ultraviolet printer, characterized in that: The method comprises: Printing transferable complex polymer patterns using UV printers; transferring the complex polymer pattern onto one of the surfaces of the active metal or alloy film; Using a polymer spraying tool, spraying a layer of polymer film of a predetermined thickness on an area without a complex polymer pattern on the surface of the active metal or alloy film on which the complex polymer pattern is attached; The acid solution is atomized by an electric spray head and sprayed onto the surface of the active metal or alloy film to which no complex polymer pattern is attached, and an infrared thermal imager is used to take pictures to obtain a specific infrared visual pattern.
2. The method according to claim 1, characterized in that Print transferable complex polymer patterns using UV printers, including: The UV-curable polymer is printed onto the adhesive surface of the polyethylene terephthalate transfer film by a UV printer and cured by ultraviolet light to eventually form a transferable polymer pattern, on which coatings of different colors are then printed to produce visible light features.
3. The method according to claim 1, characterized in that Transferring the polymer pattern onto one of the surfaces of the active metal or alloy film comprises: The ethylene terephthalate release film with the adhesive side is peeled off, and then the adhesive side is adhered to the active metal or alloy film; the ethylene terephthalate film on the other side is peeled off, leaving a complex polymer pattern on the active metal or alloy film.
4. The method according to claim 1, characterized in that: The acid solution is atomized by an electric spray head and sprayed onto the surface of the active metal or alloy film where no polymer pattern is attached. At the same time, an infrared thermal imager is used to take pictures to obtain a specific infrared visual pattern, including: Using a device to unfold an active metal or alloy film with a specific polymer pattern, and fix the active metal or alloy film on a frame; An electric atomizing nozzle is used to atomize the acid solution and spray it onto the surface of the active metal or alloy film where no polymer pattern is attached; at the same time, an infrared thermal imager is used to observe the surface of the active metal or alloy film where the polymer pattern is attached to obtain a specific infrared visual pattern.
5. The method according to claim 4, characterized in that The method also includes: if it is necessary to prepare an infrared visual pattern larger than the area of a single active metal or alloy film, multiple active metal or alloy films are spliced together, and multiple electric atomization nozzles are deployed to expand the coverage.
6. The method according to claim 1, characterized in that The acidic solution is dilute hydrochloric acid, dilute sulfuric acid, dilute nitric acid or acetic acid.
7. The method according to claim 1, characterized in that The temperature of the heating process can be precisely controlled by adjusting the spraying time of the atomized acid solution, the concentration of the acid solution or the power and spraying pattern of the electric spray head.
8. A method for preparing and realizing a physical domain infrared visual pattern based on a mask, characterized in that: The method comprises: Making a mask of the target object; Placing the mask plate on one surface of the active metal or alloy film, and coating the polymer coating on the surface of the active metal or alloy film by scraping or spraying to obtain an active metal or alloy film coated with a polymer pattern; Using a polymer spraying tool, spraying a polymer film of a predetermined thickness on an area without a polymer pattern on the surface of the active metal or alloy film coated with the polymer coating; The acid solution is atomized by an electric spray head and sprayed onto the surface of the active metal or alloy film that is not coated with a polymer pattern, and an infrared thermal imager is used to take pictures to obtain a specific infrared visual pattern.
9. The method according to claim 8, characterized in that The method also includes: if it is necessary to prepare a visual infrared pattern larger than the area of a single active metal or alloy film, multiple active metal or alloy films are spliced together and multiple electric atomizing nozzles are deployed to expand the coverage.
10. The method according to claim 8, characterized in that The temperature of the heating process can be precisely controlled by adjusting the spraying time of the atomized acid solution, the concentration of the acid solution or the power and spraying pattern of the electric spray head.