Method for accelerating corrosion test of steel structure

By spraying zinc-aluminum alloy and organic coatings, combined with dry and wet chambers and manual intervention, the accelerated corrosion test of steel structures in coastal environments has been achieved, and the corrosion problems of steel structures in high temperature, high humidity, and high salt spray environments have been solved. , providing a fast and accurate test method to help evaluate changes in mechanical properties and anti-corrosion strategies of steel.

CN118837280APending Publication Date: 2024-10-25CHINA CONSTR EIGHT ENG DIV CORP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410879119.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Steel structures are corroded to varying degrees in coastal high-temperature, high-humidity and high-salt-spray environments, resulting in a decline in mechanical properties and an increased risk of safety accidents. It is difficult to effectively speed up the corrosion test process with existing technology.

Method used

A multi-step steel structure accelerated corrosion and rust test method is adopted, including spraying zinc-aluminum alloy and organic coating, using a dry and wet chamber to provide an alternating dry and wet environment, and controlling the corrosion test through manual intervention in the corrosion test, combined with corrosion rate and mechanical property testing. Data accuracy.

Benefits of technology

It significantly speeds up the corrosion test process of steel structures, improves the accuracy and speed of test data, simplifies the operation process, provides a method to quickly obtain changes in steel properties, and helps formulate effective anti-corrosion measures.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a steel structure accelerated corrosion test method, and relates to the technical field of steel structures, and the method comprises the following steps: 1, providing a plurality of steel structures as test pieces, grouping the test pieces to form at least two groups, each group having a plurality of test pieces, the method comprises the following steps: step 1, preparing a plurality of groups of test pieces, step 2, spraying zinc-aluminum alloy on the surface of each test piece to form a zinc-aluminum alloy coating, step 3, spraying organic paint on the surface of each test piece to form an organic coating, and step 4, performing corresponding manual intervention corrosion test on each group, and spraying on the surface of the steel member in a manual intervention manner to form a corrosion test. The corrosion test on the surface of the steel member can be accelerated by using atmospheric acid and atmospheric salt in the nature, the corrosion effect on the surface of the steel member is accelerated, the obtained corrosion test data is more accurate by controlling the clear number of days and the construction brushing times, and the surface of the steel member is subjected to rapid wetting-drying alternation through the constant-temperature wetting-drying test box, so that the corrosion test efficiency is improved. The corrosion test of the steel member is accelerated and the test time is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of steel structures, in particular to a method for testing accelerated corrosion and rusting of steel structures. Background Art

[0002] Steel structures are widely used in modern engineering. At present, a large number of steel structures are needed in medical, gymnasium and other buildings in coastal areas of China. However, these steel structures are exposed to the atmospheric environment for a long time. Under the influence of the harsh environment of high temperature, high humidity and high salt fog in the coastal areas, they are all subject to varying degrees of corrosion. Corrosion will significantly reduce the strength, plasticity, toughness and other mechanical properties of metal materials, and some local corrosion such as pitting corrosion or sudden stress corrosion cracking can easily cause safety accidents. Therefore, it is necessary to do a good job in the corrosion protection of steel structures in coastal climate environments. In order to do this, we propose a method for accelerating corrosion and rust test of steel structures, conduct corrosion tests on steel, understand the performance of steel after corrosion, and provide an important basis for the corrosion protection of steel. Summary of the invention

[0003] The purpose of the present invention is to overcome the defects of the prior art and provide a method for accelerating corrosion and rust testing of steel structures, so as to solve the problem that the existing steel structures are exposed to the atmospheric environment for a long time and are affected by the harsh environment of high temperature, high humidity and high salt fog in the coastal area, and are all subject to corrosion to varying degrees. The corrosion will significantly reduce the strength, plasticity, toughness and other mechanical properties of the metal materials, and some local corrosion such as pitting corrosion or sudden stress corrosion cracking can easily cause safety accidents.

[0004] The technical solution to achieve the above object is: a method for accelerating corrosion and rust testing of steel structures, comprising the following steps:

[0005] Step 1: provide a plurality of steel structures as test pieces, and group the test pieces into at least two groups, each group having a plurality of test pieces;

[0006] Step 2: spraying zinc-aluminum alloy on the surface of each test piece to form a zinc-aluminum alloy coating;

[0007] Step 3: spraying an organic coating on the surface of each test piece to form an organic coating;

[0008] Step 4: Conduct corresponding artificial intervention corrosion tests on each group to obtain the test results of the corresponding specimens.

[0009] The technical solution of the present invention is further improved in that: the method of manually intervening in the corrosion test in step 4 is as follows:

[0010] S1: placing at least two groups into corresponding dry and wet boxes, and using the dry and wet boxes to provide a dry and wet alternating test environment for the specimens;

[0011] S2: Soak one of the grouped specimens in a saturated sodium chloride solution every 4 to 6 days until the surface is completely wetted. Each soaking lasts 1 to 3 minutes. After soaking, put it back into the dry and wet chamber.

[0012] S3: Immerse the test pieces in another group in hydrochloric acid solution every 4 to 6 days to completely wet the surface. Each immersion lasts for 1 to 3 minutes. After the immersion is completed, put them back into the dry and wet chamber.

[0013] S4: According to the set test duration, the corresponding test pieces in the dry and wet chambers are taken out regularly, and the corrosion results of the test pieces are analyzed to obtain corresponding corrosion data.

[0014] The technical solution of the present invention is further improved in that: the uniaxial tensile test steps based on the specimen in S4 are as follows:

[0015] Analyzing the corrosion results of the test piece to obtain corresponding corrosion data includes the following steps: calculating the corrosion rate of the test piece to obtain the corrosion data.

[0016] The technical solution of the present invention is further improved in that the corrosion rate of the test piece is calculated according to the corrosion rate formula, and the corrosion rate formula is as follows: test piece corrosion rate = (AB) / A×100%, wherein A is the initial thickness and B is the thickness after corrosion.

[0017] The technical solution of the present invention is further improved in that: analyzing the corrosion results of the test piece to obtain corresponding corrosion data includes the following steps:

[0018] A tensile test is performed on the specimen to obtain the corresponding yield strength parameters, ultimate strength parameters and elongation parameters of the specimen.

[0019] The technical solution of the present invention is further improved in that: the concentration of the hydrochloric acid solution in S3 for corrosion test is configured to be 16%-20%.

[0020] The technical solution of the present invention is further improved in that: the spraying method for preparing the zinc-aluminum alloy coating in step 2 adopts vertical cross spraying, and the spray gun is in a vertical direction to the base steel structure.

[0021] The technical solution of the present invention is further improved in that: when preparing the organic coating in step three, pre-coating is first performed manually for complex structures.

[0022] The technical solution of the present invention is further improved in that: the organic coating in step three can also be prepared by airless spraying.

[0023] By using the above technical solution, the present invention has the following technical effects compared with the prior art:

[0024] The present invention provides a method for accelerating corrosion and rust testing of steel structures. By means of artificial intervention, spraying is performed on the surface of steel components, and atmospheric acids and atmospheric salts in nature can be used to accelerate the corrosion test on the surface of steel components, thereby accelerating the corrosion effect on the surface of steel components. By clearly controlling the number of days and the number of times of construction and painting, the obtained corrosion test data can be made more accurate.

[0025] The invention provides a method for accelerating corrosion and rust testing of steel structures. The method uses a constant temperature dry-wet test box to perform rapid dry-wet alternation on the surface of a steel component, thereby accelerating the corrosion test of the steel component and reducing the test time.

[0026] The invention provides a method for testing accelerated corrosion and rust of steel structures. Before preparing a coating, dust and debris on the surface of a component are blown away by an air compressor to make the surface of the component cleaner.

[0027] The present invention provides a method for testing accelerated corrosion and rust of steel structures. By performing contour scanning on the surface of a component, the contour of the surface of the steel component after rust treatment can be compared with that before treatment, so that the effect of the steel structure test method can be observed more intuitively.

[0028] The invention provides a steel structure accelerated corrosion and rust test method by combining test parameters with contour scanning data. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with specific embodiments.

[0030] The present invention provides a steel structure accelerated corrosion and rust test method, which can be simpler to operate and obtain results faster than the existing technology, and provides a practical method for studying the performance of steel structures. The steel structure accelerated corrosion and rust test method is described below.

[0031] The accelerated corrosion and rust test method of the steel structure of the present invention is described below.

[0032] The present invention provides a method for accelerating corrosion and rust testing of steel structures, comprising the following steps: step one: providing a plurality of steel structures as test pieces, grouping the test pieces into at least two groups, each group having a plurality of test pieces, step two: spraying a zinc-aluminum alloy on the surface of each test piece to form a zinc-aluminum alloy coating, step three: spraying an organic coating on the surface of each test piece to form an organic coating, and step four: performing a corresponding artificial intervention corrosion test on each group, thereby obtaining a test result of the corresponding test piece.

[0033] Preferably, in addition to the at least two groups, there is another group without any coating placed in a corresponding dry and wet box for corrosion testing, so as to reflect the corrosion comparison between the coated and uncoated groups.

[0034] Furthermore, in step 2, the total thickness of the alloy coating is not less than 120 μm, and it is sprayed in two passes, the first pass is 65 μm, and the second pass is sprayed to 120 μm. The process parameters for preparing the zinc-aluminum alloy coating in step 2 are as follows: spraying voltage 25 V; spraying current 40-400 A; spraying air pressure 0.6 MPa; compressed air flow ≥16 m3 / min; spraying distance between 200 mm; spraying angle of 75°; spraying trajectory overlap range of 1 / 4-1 / 3; spray gun moving speed of 110 cm / min.

[0035] Furthermore, when spraying organic coatings on the surface of each test piece, within the time specified by the coating technical requirements, 120μm of epoxy micaceous iron intermediate paint was sprayed, 50μm of epoxy sealing paint was applied, 40μm of polyurethane topcoat was sprayed, and 40μm of fluorocarbon topcoat was sprayed.

[0036] In a specific embodiment of the present invention, the method of manually intervening in the corrosion test in step 4 is as follows: S1: placing at least two groups divided into corresponding dry-wet boxes, and using the dry-wet box to provide a dry-wet alternating test environment for the specimens, S2: immersing the specimens of one of the groups in a saturated sodium chloride solution every 4 to 6 days until the surface is completely wetted, each immersion time is 2 minutes, and the specimens are put back into the dry-wet box after the immersion is completed, S3: immersing the specimens of another group in a hydrochloric acid solution every 4 to 6 days until the surface is completely wetted, each immersion time is 2 minutes, and the specimens are put back into the dry-wet box after the immersion is completed, S4: according to the set test time, regularly take out the corresponding specimens in the dry-wet box, and analyze the corrosion results of the specimens to obtain corresponding corrosion data.

[0037] Preferably, the dry-wet alternation in S1 is to use a dry-wet box to control the humidity of the internal space so that it alternates between wet and dry. This method will quickly form a water film on the surface of the specimen, and the corrosion rate is fastest in this state.

[0038] Furthermore, the model of the dry and wet test chamber is DIIS-010.

[0039] Furthermore, the test duration is set to 30 days, that is, a specimen is taken out from each group every 30 days to check the corrosion condition, and the specimens in each group are compared. The number of specimens in each group is at least 6, so the total test time is 6 months, one specimen is taken out every month, and the corrosion results of the specimens are analyzed to obtain corrosion data.

[0040] In a specific embodiment of the present invention, analyzing the corrosion results of the test piece to obtain corresponding corrosion data includes the following steps: calculating the corrosion rate of the test piece to obtain the corrosion data.

[0041] Furthermore, analyzing the corrosion results of the test piece to obtain corresponding corrosion data also includes the following steps:

[0042] A tensile test is performed on the specimen to obtain the corresponding yield strength parameters, ultimate strength parameters and elongation parameters of the specimen.

[0043] Furthermore, analyzing the corrosion results of the test piece to obtain corresponding corrosion data also includes the following steps:

[0044] The pits on the surface of the specimen are scanned and detected to obtain the pit data.

[0045] Specifically, the degradation of mechanical properties of corroded components is studied, and comparisons are made under different environments. Combined with the measured corrosion rate and parameters for evaluating surface morphology, the relationship between corrosion and changes in mechanical properties of components is explored, and a model for the degradation of mechanical properties of steel under different environments is established;

[0046] Based on the corrosion law of steel structures under different environmental conditions, the quantitative relationship between the corrosion rate of steel and time under different corrosion conditions is established;

[0047] In view of the fact that the corrosion pits on the surface of the corroded specimens are very random, the surface profile of the corroded specimens was measured with the help of a surface roughness detector, and a characterization method for the corrosion pits on the surface of corroded steel structures was established using fractal theory.

[0048] Through the tensile material performance test of corroded specimens, the influence of corrosion degree and corrosion type (surface condition of corroded specimens) on the mechanical properties of steel such as yield strength, ultimate strength and elongation was explored, and the quantitative relationship between corrosion degree and mechanical properties of steel was established.

[0049] Furthermore, the surface morphology of steel includes four aspects: roughness, waviness, shape error and surface texture of the component surface. The roughness of the two-dimensional profile of the surface of the corroded specimen is measured using a roughness measuring instrument.

[0050] Furthermore, the roughness measuring instrument model is TR300.

[0051] Furthermore, the traces left by the probe on both sides of the specimen sampling length are recorded by computer, which is the waviness of the steel plate surface. Several scanning tracks are customized on the color optical image, and the surface texture of the scanning area is obtained by scanning the 2D true color image.

[0052] In a specific embodiment of the present invention, the corrosion rate of the specimen is calculated according to the corrosion rate formula, and the corrosion rate formula is as follows: specimen corrosion rate = (AB) / A×100%, wherein A is the initial thickness and B is the thickness after corrosion.

[0053] In a specific embodiment of the present invention, the spraying method for preparing the zinc-aluminum alloy coating in step 2 adopts vertical cross spraying.

[0054] Furthermore, when spraying, the next spraying can be carried out 15 minutes after each spraying is completed.

[0055] Furthermore, the spray gun is perpendicular to the base steel structure. When vertical spraying is not possible, the inclination between the spray gun and the workpiece is not less than 45°. When spraying zinc-aluminum alloy coating on a large area, divide the working area into several small areas, adjust the spraying spark beam angle to less than 40°, and the spray beam width to 3-4cm.

[0056] In a specific embodiment of the present invention, when preparing the organic coating in step three, pre-coating is first performed manually for complex structures, and the organic coating is prepared in step three by airless spraying with a spraying pressure of 0.4MPa-0.5MPa.

[0057] In a specific embodiment of the present invention, the hydrochloric acid solution in S3 is configured to have a corrosion test concentration of 18%.

[0058] The beneficial effects of the steel structure accelerated corrosion and rust test method of the present invention are:

[0059] The present invention is designed to conduct corrosion and rust tests on steel materials, establish a set of steel structure coating construction processes, and clarify the number of coating times, processes and corresponding construction management methods.

[0060] Establish a set of recommendations for various indicators such as viscosity, fineness, impact resistance, hardness, drying time, etc. for steel structure anti-corrosion coatings.

[0061] Clarify the surface treatment requirements and paint film coating management of steel structures during the construction process, and propose corresponding construction plans for different coating environments.

[0062] Compared with existing technologies, this test method is simpler to operate, has faster results, and provides a practical method for studying the performance of steel structures.

[0063] The present invention is described in detail above in conjunction with the embodiments, and those skilled in the art can make various variations of the present invention according to the above description. Therefore, certain details in the embodiments should not constitute limitations of the present invention, and the scope of protection of the present invention shall be defined by the scope of the attached claims.

Claims

1. A method for testing accelerated corrosion and rust of steel structures, characterized in that: The following steps are involved: Step 1: provide a plurality of steel structures as test pieces, and group the test pieces into at least two groups, each group having a plurality of test pieces; Step 2: spraying zinc-aluminum alloy on the surface of each test piece to form a zinc-aluminum alloy coating; Step 3: spraying an organic coating on the surface of each test piece to form an organic coating; Step 4: Conduct corresponding artificial intervention corrosion tests on each group to obtain the test results of the corresponding specimens.

2. A steel structure accelerated corrosion test method according to claim 1, characterized in that: The method of manually intervening in the corrosion test in step 4 is as follows: S1: placing at least two groups into corresponding dry and wet boxes, and using the dry and wet boxes to provide a dry and wet alternating test environment for the specimens; S2: Soak one of the grouped specimens in a saturated sodium chloride solution every 4 to 6 days until the surface is completely wetted. Each soaking lasts 1 to 3 minutes. After soaking, put it back into the dry and wet chamber. S3: Immerse the test pieces in another group in hydrochloric acid solution every 4 to 6 days to completely wet the surface. Each immersion lasts for 1 to 3 minutes. After the immersion is completed, put them back into the dry and wet chamber. S4: According to the set test duration, the corresponding test pieces in the dry and wet chambers are taken out regularly, and the corrosion results of the test pieces are analyzed to obtain corresponding corrosion data.

3. A steel structure accelerated corrosion and rust test method according to claim 2, characterized in that: Analyzing the corrosion results of the test piece to obtain corresponding corrosion data includes the following steps: calculating the corrosion rate of the test piece to obtain the corrosion data.

4. A steel structure accelerated corrosion and rust test method according to claim 3, characterized in that: The corrosion rate of the test piece is calculated according to the corrosion rate formula, and the corrosion rate formula is as follows: test piece corrosion rate = (AB) / A×100%, wherein A is the initial thickness and B is the thickness after corrosion.

5. A steel structure accelerated corrosion test method according to claim 2, characterized in that: Analyzing the corrosion results of the specimen to obtain the corresponding corrosion data includes the following steps: A tensile test is performed on the specimen to obtain the corresponding yield strength parameters, ultimate strength parameters and elongation parameters of the specimen.

6. A steel structure accelerated corrosion and rust test method according to claim 2, characterized in that: The hydrochloric acid solution in S3 is configured to have a concentration of 16%-20% in the corrosion test.

7. A steel structure accelerated corrosion and rust testing method according to claim 1, characterized in that: The spraying method for preparing the zinc-aluminum alloy coating in step 2 is vertical cross spraying.

8. A steel structure accelerated corrosion and rust testing method according to claim 1, characterized in that: When preparing the organic coating in step 3, pre-coating is first performed manually for complex structures.

9. A steel structure accelerated corrosion and rust testing method according to claim 1, characterized in that: In the step 3, the organic coating is prepared by airless spraying.