Sodium-ion battery hard carbon negative electrode material and preparation method thereof
Through ozone activation of the cross-linking reaction between alkaline lignin and phenolic resin, a three-dimensional conductive network is formed, which solves the problem of poor rate performance of hard carbon materials at high current densities and achieves high electrochemical performance of hard carbon anode materials for sodium ion batteries. and cyclic stability.
Patent Information
- Application Number
- CN202410854219.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Existing hard carbon materials based on phenolic resin and lignin have poor rate performance at large current densities and insufficient cycle stability, making them unable to meet the commercial needs of sodium-ion batteries.
Ozone is used to activate alkaline lignin to form a three-dimensional conductive network on the surface of phenolic resin spheres. The hard carbon negative electrode material for sodium ion batteries is obtained through high-temperature carbonization. Ozone is used to activate lignin to introduce highly reactive hydroxyl radicals to cross-link with the phenolic resin. , forming C=O sodium storage active sites and a three-dimensional conductive network.
It significantly improves the reversible capacity and rate performance of hard carbon anode materials for sodium-ion batteries, ensures cycle stability under high current density, and improves the electrochemical performance of sodium-ion batteries.
Smart Images

Figure CN118841544A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion battery hard carbon negative electrode material and a preparation method thereof. Background Art
[0002] With the advancement of science and technology and the expansion of social population, human society has an increasing demand for environmentally friendly new energy. In response to this problem, researchers have proposed a variety of new energy sources in recent years. Lithium-ion batteries have become the most widely used rechargeable batteries due to their excellent electrochemical properties. However, the content of lithium in nature is low and unevenly distributed, which to a large extent restricts the further large-scale application of lithium-ion batteries. In the era of "beyond lithium-ion batteries", rechargeable sodium-ion batteries have become an important energy storage technology due to their low cost, high sodium abundance, and wide distribution of sodium resources. They are widely used in renewable energy integration, electric vehicles, and energy storage systems. As a key component of sodium-ion batteries, negative electrode materials play an important role in the development of sodium-ion batteries. However, Na + Radius Bili + Radius Larger and Na + The thermodynamic instability of graphite anodes has hampered the development and application of sodium-ion batteries. This limitation has triggered a lot of efforts to develop a large number of advanced sodium-ion battery anode materials.
[0003] Hard carbon negative electrode materials have attracted extensive attention from researchers due to their advantages such as wide sources of precursors, simple preparation process, environmental friendliness, high safety and low cost. The main factors affecting the electrochemical performance of hard carbon negative electrode materials are graphite layer spacing, pore structure, heteroatom doping and defects. Among them, the pore structure and heteroatom doping have a more significant impact on the electrochemical performance of hard carbon negative electrode materials. Creating a certain number of pore structures in the material can improve the reversible capacity of the material and accelerate Na + The adsorption and desorption rates of Na can be accelerated by introducing suitable heteroatoms. + adsorption process, thereby improving the rate performance and reversible capacity of the material.
[0004] The main scientific problems of traditional phenolic resin hard carbon negative electrode materials are: insufficient conductivity, poor rate performance, etc. Therefore, it is necessary to develop an improved method for preparing hard carbon negative electrode materials to overcome the above problems and improve the performance and energy density of sodium ion batteries. Huang Yujie et al. used polyimide as a precursor and rationally designed carbon nanodots to obtain a hard carbon negative electrode material with a rich pore structure. The material has a good conductivity at 0.1Ag. -1 The current density is 220 mAh g -1The reversible specific capacity of the material was 100%, and there was no obvious capacity decay after 125 cycles (Advanced Functional Materials.2023,2308392). Zheng Zhi et al. used starch as a carbon source and synthesized a hard carbon material with a large number of pores by CO2 etching. The material was -1 320mAh g -1 The reversible specific capacity at 0.8Ag -1 It has 171mAh g -1 Wu Dongyang et al. used boric acid and glucose as boron source and carbon source to obtain boron-doped hard carbon materials, which have a capacity of 1Ag -1 The current density is 80 mAh g -1 (Journal of Materials Chemistry A.2022,10,17225). However, the above materials have a low capacity of 2Ag -1 The capacity at the current density is 100 mAh g -1 However, the poor rate performance cannot meet the commercialization requirements of the battery.
[0005] There are many reports in the prior art on the use of phenolic resin and lignin as carbon sources to prepare hard carbon materials. For example, CN117326546A, CN116395668A, CN116969441A, CN114044508A, and CN108217623A. However, lignin only serves as a carbon source and cannot fully utilize the characteristics of lignin in that it is easy to form hydroxyl radicals with high reactivity, resulting in the electrochemical performance of the obtained hard carbon material still needs to be improved. Summary of the invention
[0006] In order to solve the defects of poor rate performance of hard carbon materials prepared based on phenolic resin and lignin in the prior art, and the inability to meet the requirements of capacity and cycle stability at a large current density, the present invention proposes an improved strategy of using ozone to activate alkaline lignin and constructing it on the surface of phenolic resin spheres to form a three-dimensional conductive network. The present invention provides the following technical solutions to solve the above technical problems:
[0007] A sodium ion battery negative electrode material is a three-dimensional network structure of lignin-based carbon coated on the surface of phenolic resin-based carbon. The sodium ion battery negative electrode material is obtained by high-temperature carbonization of phenolic resin and ozone-activated alkaline lignin as carbon sources. The ozone-activated alkaline lignin is obtained by placing alkaline lignin in an ozone atmosphere and activating it at room temperature.
[0008] Furthermore, the alkaline lignin is placed in an ozone atmosphere for activation time of 3-10 hours, preferably 4-6 hours.
[0009] Further, the ozone-activated alkaline lignin accounts for 30-50% of the total mass of the ozone-activated alkaline lignin and the phenolic resin.
[0010] The present invention also provides a method for preparing the above-mentioned sodium ion battery negative electrode material, comprising the following steps:
[0011] (S1) placing alkaline lignin in a reactor, connecting the reactor to an ozone generator, introducing ozone gas into the reactor, and performing ozone activation on the alkaline lignin at room temperature;
[0012] (S2) uniformly mixing phenolic resin and ozone-activated alkaline lignin, and placing the mixture in a muffle furnace for pre-oxidation;
[0013] (S3) placing the pre-oxidized mixture in a tubular furnace, performing low-temperature pre-carbonization and high-temperature carbonization under an inert gas atmosphere to obtain the desired hard carbon negative electrode material for a sodium ion battery.
[0014] The preparation of phenolic resin is well known in the art, and it is obtained by polymerizing diphenol compounds and formaldehyde. For example, in one specific embodiment of the present invention, resorcinol is placed in an alcohol aqueous solution and ultrasonically dissolved, deionized water and ammonia water are added to the resulting solution under stirring conditions, and then formaldehyde is added. After continuous stirring, the solution is centrifuged and dried to obtain the phenolic resin.
[0015] Furthermore, the volume mass ratio of formaldehyde solution to resorcinol is (1-2) mL:1 g; formaldehyde is added in the form of formaldehyde aqueous solution, and the formaldehyde mass concentration is 30-40 wt %; and the concentration of ammonia aqueous solution is 20-30%.
[0016] Further, in step (S1), the ratio of the flow rate of ozone to the mass of alkaline lignin is 0.3-0.5L / min / kg, and the time of ozone activation should be controlled within 3-10h, preferably 4-6h. By adjusting the ozone activation time, the degree of ozonation of alkaline lignin can be controlled, and the degree of ozonation should be controlled within a suitable range. If the degree of ozonation is too high, the alkaline lignin will be over-oxidized, thereby reducing its cross-linking activity. If the degree of ozonation is too low, the degree of oxidation will be insufficient, and sufficient active reaction functional groups cannot be generated, which is not conducive to the cross-linking reaction of lignin and phenolic resin.
[0017] Furthermore, in step (S2), the ozone-activated alkaline lignin accounts for 30-50% of the total mass of the ozone-activated alkaline lignin and the phenolic resin, and the uniform mixing method is ball milling and a high-speed mixer.
[0018] Furthermore, in step (S2), the pre-oxidation temperature should be controlled at 200-300°C, and the pre-oxidation time should be 3-5h.
[0019] Further, in step (S3), the inert atmosphere is nitrogen and / or argon, the heating rate is 1-5°C / min, the low-temperature pre-carbonization is treated at 350°C-500°C for 1-3h, and the high-temperature carbonization is treated at 1200-1500°C for 2-5h. Low-temperature retention carbonization can effectively promote the release of small molecular substances in the material, form sufficient pore structures inside and on the surface of the material, and facilitate the storage and transportation of sodium ions.
[0020] The present invention achieves the following beneficial technical effects:
[0021] The present invention adopts the strategy of ozone-activated modified lignin to introduce highly reactive hydroxyl radicals into the interior of the lignin, and allows them to undergo a cross-linking reaction with the phenolic hydroxyl groups on the phenolic resin, thereby forming a C=O sodium storage active site and uniformly constructing a three-dimensional conductive network on the surface of the phenolic sphere, so that the hard carbon material has excellent reversible capacity and rate, further improving the electrochemical performance of sodium-ion batteries, and is expected to promote the development and application of sodium-ion batteries.
[0022] The raw materials required for the sodium ion battery hard carbon negative electrode material synthesized by the present invention are low in price and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a scanning electron microscope image of the hard carbon negative electrode material for the sodium ion battery in Example 1.
[0024] Figure 2 This is a transmission electron microscope image of the porous hollow carbon ball negative electrode material particles prepared in Example 1.
[0025] Figure 3 This is a high-resolution transmission electron micrograph of the porous hollow carbon sphere negative electrode material particles prepared in Example 1.
[0026] Figure 4 This is a scanning electron microscope image of the hard carbon negative electrode material for the sodium ion battery in Comparative Example 1.
[0027] Figure 5 This is a charge and discharge curve diagram of the sodium ion battery hard carbon negative electrode material in Example 1.
[0028] Figure 6 This is a performance diagram of the battery capacity retention rate at different current densities in Example 1. DETAILED DESCRIPTION
[0029] To make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be described in detail below. The following examples are convenient for better understanding of the present invention, but are not intended to limit the present invention. The experimental methods in the following examples are conventional methods unless otherwise specified.
[0030] Example 1
[0031] (1) Preparation of negative electrode materials
[0032] 3kg of resorcinol was dissolved in 100L of a 9:1 mixture of ethanol and water, and stirred and dissolved on a magnetic stirrer at 400rmp. Then 18L of ammonia water (29wt%) and 4.L of formaldehyde (40wt%) were slowly added to the above solution in sequence to induce polymerization. After the above mixture was stirred continuously for 24h, the obtained phenolic resin microspheres were centrifuged, washed with deionized water and ethanol, and then dried. Alkaline lignin was placed in a reactor, and the reactor was connected to an ozone generator. The ratio of ozone flow rate to alkaline lignin mass was adjusted to 0.3L / min / kg, and it was taken out after activation in an ozone atmosphere for 4h. Phenolic resin and ozone-activated alkaline lignin were hand-milled for 20min at a mass ratio of 7:3 and fully mixed. The mixture was placed in a muffle furnace and pre-oxidized at 300℃ for 5h at a heating rate of 2℃ / min to obtain an intermediate. Subsequently, the intermediate was heated to 450°C at a heating rate of 2°C / min in an Ar atmosphere and kept at this temperature for 2 hours. Thereafter, the temperature was further increased to 1400°C and carbonized for 3 hours to obtain the desired hard carbon material.
[0033] (2) Preparation of negative electrode sheet
[0034] The negative electrode material obtained in step (1), the conductive additive Super P, and the binder PVDF were mixed in weight proportions of 90 parts, 5 parts, and 5 parts, dissolved in the solvent NMP, and stirred to obtain a uniform slurry. The slurry was then evenly coated on a carbon-coated copper foil using a 75 μm scraper, dried, and sliced to obtain a negative electrode sheet.
[0035] (3) Assembling sodium ion batteries
[0036] The prepared negative electrode sheet was assembled into a sodium ion battery with a metallic sodium negative electrode. The electrolyte was 1 M sodium hexafluorophosphate (NaPF6) dissolved in diethylene glycol dimethyl ether (DEGDME). The diaphragm was a porous glass fiber diaphragm (Whatman, GF / D). The button cells were assembled and electrochemical tests were performed in an argon glove box with a water oxygen value below 0.1 ppm. The electrochemical performance tests were carried out on a NEWAREBTS-4000 battery testing system at room temperature of 25°C.
[0037] Example 3
[0038] Other conditions are the same as those in Example 1, except that in step (1), the mass ratio of phenolic resin to ozone-activated alkaline lignin is 1:1.
[0039] Example 4
[0040] The other conditions are the same as those in Example 1, except that in step (1), the mass ratio of phenolic resin to ozone-activated alkaline lignin is 7:3.
[0041] Example 5
[0042] The other conditions are the same as those in Example 1, except that in step (1), the mass ratio of phenolic resin to ozone-activated alkaline lignin is 2:8.
[0043] Example 6
[0044] The other conditions were the same as those in Example 1, except that in step (1), the alkaline lignin was placed in the ozone atmosphere for 6 h.
[0045] Example 7
[0046] The other conditions were the same as those in Example 1, except that in step (1), the alkaline lignin was placed in the ozone atmosphere for 3 h.
[0047] Example 8
[0048] The other conditions are the same as those in Example 1, except that in step (1), the time for which the alkaline lignin is placed in the ozone atmosphere is not 10 h.
[0049] Comparative Example 1
[0050] The other conditions are the same as those in Example 1, except that in step (1), the alkaline lignin is replaced by crystalline cellulose.
[0051] Comparative Example 2
[0052] The other conditions are the same as those in Example 1, except that in step (1), the alkaline lignin is replaced by hemicellulose.
[0053] Comparative Example 3
[0054] The other conditions are the same as those in Example 1, except that in step (1), the ozone-activated alkaline lignin is replaced by an alkaline lignin of equal mass, that is, the alkaline lignin is not ozone-activated.
[0055] Application Examples Electrochemical performance test
[0056] The sodium ion batteries prepared in the above examples and comparative examples were subjected to rate performance tests: the test voltage was between 0.001-3V, and the test voltage was between 0.05, 0.1, 0.5, and 1Ag. -1The specific capacity at the current density is shown in Table 1 below.
[0057] Table 1 Sodium ion battery rate performance data
[0058]
[0059]
[0060] From the above results, it can be seen that the sodium ion battery hard carbon negative electrode material prepared by the present invention has good electrochemical performance, excellent rate performance and cycle stability, indicating that the present invention selects the self-synthesized phenolic resin and ozone-activated alkaline lignin to mix for pre-oxidation to induce the simultaneous production of C=O cross-linked structure and three-dimensional conductive network coating is successful. The hard carbon negative electrode material prepared by the present invention is a solid sphere with a diameter of about 1 μm, which is not prone to structural damage during the cycle, thereby making it have good cycle stability. The present invention uses ozone-activated alkaline lignin as a cross-linking agent. During the pre-oxidation process, the phenolic resin and it not only produce cross-linking to obtain more C=O sodium storage active functional groups, but also are coated with a layer of three-dimensional conductive network, so that the material can increase the sodium ion diffusion rate and promote electron transfer without losing the capacity of the material, thereby making the material have good rate performance and capacity retention rate. At 1Ag -1 At a current density of 1.34 W, its capacity is still as high as 312 mAh g -1 , the capacity retention rate after 200 cycles is 92.6%.
[0061] Figure 1 This is a scanning electron microscope image of the hard carbon negative electrode material for a sodium ion battery obtained in Example 1. It can be seen from the figure that the surface of the synthesized negative electrode material is successfully coated with a three-dimensional conductive network, and the coating of the network is formed by the cross-linking reaction between the hydroxyl groups in the phenolic resin and the hydroxyl radicals in the activated lignin. During the pre-oxidation process, the cross-linking reaction causes the overflow of small molecules, thereby forming a large number of pore structures, which is beneficial to the diffusion of sodium ions during the battery charging and discharging process, and can greatly improve the rate performance of the sodium ion battery. In addition, the structure of the solid hard carbon sphere is relatively stable, so that the material can have good structural stability during the cycle process, thereby improving the cycle performance of the sodium ion battery.
[0062] Figure 2 This is a transmission electron microscope image of the hard carbon negative electrode material for sodium ion batteries obtained in Example 1. It can be seen from the figure that the synthesized negative electrode material has a uniformly coated three-dimensional conductive network, which is the same as the material microscopic morphology observed in the scanned image. The coating layer with high conductivity can promote the rapid transmission kinetics of sodium ions, thereby promoting the rate performance of the material; more C=O functional groups can effectively increase the reversible capacity of the material.
[0063] Figure 3 This is a high-resolution transmission electron microscope image of the hard carbon negative electrode material for sodium ion batteries. It can be seen from the figure that the surface of the synthesized negative electrode material has a high degree of graphitization and orderly lattice fringes. The high degree of graphitization on the surface of the material can provide a channel for rapid transmission of sodium ions during the charge and discharge process, thereby increasing the sodium ion transmission rate and further improving the rate performance of the material.
[0064] Figure 4 This is a scanning electron microscope image of the electrode material (Comparative Example 1) obtained by mixing alkaline lignin without ozone activation with phenolic resin, pre-oxidizing and high-temperature calcining. It can be seen from the figure that alkaline lignin without ozone activation cannot form a coating layer with phenolic resin. This is because ozone activation can introduce hydroxyl radicals with high reactivity into the interior of lignin, and make it undergo a cross-linking reaction with the phenolic hydroxyl groups on the phenolic resin, forming a C=O sodium storage active site while uniformly constructing a three-dimensional conductive network on the surface of the phenolic sphere. However, alkaline lignin without ozone activation cannot form hydroxyl radicals with high reactivity, so it cannot undergo a cross-linking reaction with phenolic resin.
[0065] Figure 5 This is a charge and discharge curve diagram of the sodium ion battery hard carbon negative electrode material in Example 1. Figure 6 This is a performance diagram of the battery capacity retention rate at different current densities in Example 1.
Claims
1. A sodium ion battery negative electrode material, characterized in that: The three-dimensional network structure of lignin-based carbon is coated on the surface of phenolic resin-based carbon. The negative electrode material of the sodium ion battery is obtained by high-temperature carbonization of phenolic resin and ozone-activated alkaline lignin as carbon sources. The ozone-activated alkaline lignin is obtained by placing alkaline lignin in an ozone atmosphere and activating it at room temperature.
2. The sodium ion battery negative electrode material according to claim 1, characterized in that The activation time of alkaline lignin in ozone atmosphere is 3-10h.
3. The sodium ion battery negative electrode material according to claim 2, characterized in that The activation time of alkaline lignin in ozone atmosphere is 4-6h.
4. The sodium ion battery negative electrode material according to claim 1, characterized in that The ozone activated alkaline lignin accounts for 30-50% of the total mass of the ozone activated alkaline lignin and the phenolic resin.
5. The method for preparing the negative electrode material for a sodium ion battery according to any one of claims 1 to 4, characterized in that: The following steps are involved: (S1) placing alkaline lignin in a reactor, connecting the reactor to an ozone generator, introducing ozone gas into the reactor, and performing ozone activation on the alkaline lignin at room temperature; (S2) uniformly mixing phenolic resin and ozone-activated alkaline lignin, and placing the mixture in a muffle furnace for pre-oxidation; (S3) placing the pre-oxidized mixture in a tubular furnace, performing low-temperature pre-carbonization and high-temperature carbonization under an inert gas atmosphere to obtain the desired hard carbon negative electrode material for a sodium ion battery.
6. The preparation method according to claim 5, characterized in that: In step (S1), the ratio of the ozone flow rate to the mass of the alkaline lignin is 0.3-0.5 L / min / kg, and the ozone activation time should be controlled within 3-10 hours.
7. The preparation method according to claim 6, characterized in that: In step (S1), the time of ozone activation should be controlled within 4-6 hours.
8. The preparation method according to claim 5, characterized in that: In step (S2), the ozone-activated alkaline lignin accounts for 30-50% of the total mass of the ozone-activated alkaline lignin and the phenolic resin, and the uniform mixing method is ball milling and a high-speed mixer.
9. The preparation method according to claim 5, characterized in that: In step (S2), the pre-oxidation temperature should be controlled at 200-300°C, and the pre-oxidation time is 3-5h.
10. The preparation method according to claim 5, characterized in that: In step (S3), the inert atmosphere is nitrogen and / or argon, the heating rate is 1-5°C / min, the low-temperature pre-carbonization is treated at 350°C-500°C for 1-3h, and the high-temperature carbonization is treated at 1200-1500°C for 2-5h.
Citation Information
Patent Citations
Method for preparing lignin-based super-capacity carbon through catalytic activation
CN115410834A
Molecular-weight-controllable oxidized lignin modified phenolic resin-based hard carbon as well as preparation method and application thereof
CN117963877A
Lignocellulose phenolic resin / doped bamboo-based porous carbon derived hard carbon composite material, preparation method and application
CN118239469A
Method for activating and precipitating lignin
US20180179339A1