Battery, positive electrode lithium supplement agent and preparation method of positive electrode lithium supplement agent

By using Li5FeO4, Li2NiO2, and Li6CoO4 as the matrix and forming a hydrophobic coating layer in the lithium battery cathode lithium replenishing agent, the performance problem of lithium powder materials under the influence of the environment is solved, and the air stability and electrochemical performance of the battery are improved. .

CN118841573AInactive Publication Date: 2024-10-25SHENZHEN BTR NEW ENERGY TECH RES INST CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410878608.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lithium-containing powder materials used as cathode lithium replenishing agents are easily affected by the environment during storage and application, resulting in unpredictable performance and electrochemical performance, especially in new energy batteries.

Method used

Matrix materials such as Li5FeO4, Li2NiO2, and Li6CoO4 are used, and a hydrophobic spherical structure is formed through a coating layer of powder material. The chemical formula is LiaMbNcRdPeTfOg. The coating layer is formed through a sintering process to improve the stability and electrochemical performance of the material.

Benefits of technology

It improves air stability and electrochemical performance, enhances the hydrophobicity and electrolyte wettability of powder materials, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118841573A_ABST
    Figure CN118841573A_ABST
Patent Text Reader

Abstract

The invention discloses a battery, a positive electrode lithium supplement agent and a preparation method thereof, and the positive electrode lithium supplement agent comprises a matrix and a coating layer; wherein the matrix is selected from at least one of Li5FeO4, Li2NiO2 and Li6CoO4, and the matrix is selected from at least one of Li2NiO2 and Li6CoO4; wherein the coating layer is made of a powder material; the chemical formula of the powder material is Li M N < c > R < d > P < e > T < f > O < g >, wherein M is selected from at least one of In, Sc, B, Ga, Nb, Y, Zr, Al, Ni, Co, Mn, Mg, Ca, Sr, Cu, Zn, Fe, Na and K; wherein N is selected from at least one of Ti, Zr, Hf, Si, Ge and Sn; wherein R is selected from at least one of Nb, Ti, Zr, Hf, As, Sb, Si, Ge and Sn, and R and N are respectively selected from different elements; wherein T is selected from at least one of S, Se, N, F, Cl, Br and I. The battery, the positive electrode lithium supplement agent and the preparation method of the positive electrode lithium supplement agent have the beneficial effects that the stability in air and the electrochemical performance can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of new energy materials, and in particular to a battery, a positive electrode lithium supplement and a preparation method thereof. Background Art

[0002] In the relevant technologies of new energy batteries, lithium-containing powder materials are used to coat the positive electrode plates; the more commonly used lithium-containing powder materials include LATP, LLZO, LLZTO, etc.

[0003] However, when these lithium-containing powder materials are used as positive electrode coating materials, they will be affected by the environment during storage, which will have unpredictable effects on the powder performance and the electrochemical performance after being applied to new energy batteries. This problem is particularly obvious when these lithium-containing powders are used as positive electrode lithium supplements. Summary of the invention

[0004] In view of this, the present application provides a battery, a positive electrode lithium supplement and a preparation method thereof, aiming to improve the existing problems.

[0005] The embodiment of the present application is implemented as follows: a positive electrode lithium supplement, the positive electrode lithium supplement comprising:

[0006] substrate and cladding;

[0007] Wherein, the matrix is ​​selected from at least one of Li5FeO4, Li2NiO2, and Li6CoO4;

[0008] Wherein, the coating layer is formed of powder material;

[0009] The chemical formula of the powder material is Li a M b N c R d P e T f O g ;

[0010] Wherein, M is selected from at least one of In, Sc, B, Ga, Nb, Y, Zr, Al, Ni, Co, Mn, Mg, Ca, Sr, Cu, Zn, Fe, Na, and K;

[0011] Wherein, N is selected from at least one of Ti, Zr, Hf, Si, Ge, and Sn;

[0012] Wherein, R is selected from at least one of Nb, Ti, Zr, Hf, As, Sb, Si, Ge, and Sn, and R and N are selected from different elements respectively;

[0013] Wherein, T is selected from at least one of S, Se, N, F, Cl, Br and I.

[0014] Optionally, in some embodiments of the present application, the primary particles and / or secondary particles of the powder material are spheroids; the spheroids have a first short axis, a second short axis and a long axis; the long axis is perpendicular to the plane where the first short axis and the second short axis are located; the dimensions of the spheroids at the first short axis, the second short axis and the long axis are x, y, z, respectively, wherein 1≤z / x<2, 1≤z / y<2.

[0015] Optionally, in some embodiments of the present application, the dimension z of the spheroid on the major axis is in the range of 0.01 μm ≤ z ≤ 100 μm.

[0016] Optionally, in some embodiments of the present application, d / (b+c+d+e) is defined as a first metrological characteristic value A; the value range of the first metrological characteristic value A is 0<A<0.6.

[0017] Optionally, in some embodiments of the present application, f / (f+g) is defined as a second metrological characteristic value B; the value range of the second metrological characteristic value B is 0<B≤0.4.

[0018] Optionally, in some embodiments of the present application, wherein the Li a M b N c R d P e T f O g , 1<a≤6, 0<b<1, 0<c<2, 0<d<3, 0<e<3, 0<f<8, 0<g<12.

[0019] Accordingly, the present application also provides a method for preparing a positive electrode lithium supplement, comprising:

[0020] Mixing the matrix of the positive electrode lithium supplement agent and the powder material for coating;

[0021] Sintering the mixed matrix and powder material;

[0022] Wherein, the matrix is ​​selected from at least one of Li5FeO4, Li2NiO2, and Li6CoO4;

[0023] Wherein, the coating layer is formed of powder material;

[0024] The chemical formula of the powder material is Li a M b N c R d P e T f Og ;

[0025] Wherein, M is selected from at least one of In, Sc, B, Ga, Nb, Y, Zr, Al, Ni, Co, Mn, Mg, Ca, Sr, Cu, Zn, Fe, Na, and K;

[0026] Wherein, N is selected from at least one of Ti, Zr, Hf, Si, Ge, and Sn;

[0027] Wherein, R is selected from at least one of Nb, Ti, Zr, Hf, As, Sb, Si, Ge, and Sn, and R and N are selected from different elements respectively;

[0028] Wherein, T is selected from at least one of S, Se, N, F, Cl, Br and I.

[0029] Optionally, in some embodiments of the present application, the sintering temperature for sintering the mixed matrix and the powder material is in the range of 200-800°C, the sintering time is 3-12h, the temperature rise rate is in the range of 1-10°C / min, and the sintering atmosphere is nitrogen.

[0030] Optionally, in some embodiments of the present application, the mass ratio of the powder material to the matrix is ​​(0.1-10):100.

[0031] Correspondingly, an embodiment of the present application further provides a battery, characterized in that: it includes the aforementioned positive electrode lithium supplement agent; and / or includes the lithium supplement agent prepared by the aforementioned preparation method.

[0032] The beneficial effects of the present application are: providing a battery, a positive electrode lithium supplement and a preparation method thereof that can improve stability under air and improve electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0034] Figure 1 This is a SEM image of a 30μm-micron-grade powder material provided in this application;

[0035] Figure 2 This is a SEM image of a 30nm-nanoscale powder material provided by the present application;

[0036] Figure 3 It is a schematic diagram of various defined axes of a powder material provided in an embodiment of the present application;

[0037] Figure 4 It is a schematic diagram of the main steps of a method for preparing a powder material provided in an embodiment of the present application;

[0038] Figure 5 It is a schematic diagram of the main steps of a method for preparing a positive electrode lithium supplement provided in an embodiment of the present application. DETAILED DESCRIPTION

[0039] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0041] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.

[0042] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0043] In the present application, "at least one" means one or more, and "plurality" means two or more. "One or more", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0044] In the present application, when a layer is formed "on" another layer, the so-called "on" is a broad concept, which may indicate that the formed another layer is adjacent to the certain layer, or may indicate that there are other spacing structural layers between the another layer and the certain layer. For example, when a second electrode is formed "on" the first carrier functional layer, the so-called "on" may indicate that the formed second electrode is adjacent to the first carrier functional layer, or may indicate that there are other spacing structural layers between the second electrode and the first carrier functional layer, such as a light-emitting layer.

[0045] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0046] The technical solution of this application is as follows:

[0047] In a first aspect, an embodiment of the present application provides a positive electrode lithium replenisher, the positive electrode lithium replenisher comprising:

[0048] substrate and cladding;

[0049] Wherein, the matrix is ​​selected from at least one of Li5FeO4, Li2NiO2, and Li6CoO4;

[0050] Wherein, the coating layer is formed by powder material.

[0051] The chemical formula of the hydrophobic powder material is Li a M b N c R d P e Tf O g ; wherein, M is selected from at least one of In, Sc, B, Ga, Nb, Y, Zr, Al, Ni, Co, Mn, Mg, Ca, Sr, Cu, Zn, Fe, Na, and K; wherein, N is selected from at least one of Ti, Zr, Hf, Si, Ge, and Sn; wherein, d / (b+c+d+e) is defined as the first metrological characteristic value A; wherein, f / (f+g) is defined as the second metrological characteristic value B; wherein the value range of the first metrological characteristic value A is 0<A<0.6; wherein the value range of the second metrological characteristic value B is 0<B≤0.4.

[0052] Based on the above scheme, the primary particles or secondary particles of the powder material of the present application have a spherical shape, so that the powder material of the present application has good hydrophobicity, which can improve the powder performance of the powder material of the present application and the electrochemical performance when specifically applied to secondary batteries. Among them, the content of T will affect the contact angle of the powder material of the present application to water and electrolyte; therefore, it is necessary to set the content of T in a more appropriate range to take into account the hydrophobicity and the performance of being wetted by the electrolyte (electrolyte affinity performance).

[0053] In some embodiments of the present application, the value range of the first metrological characteristic value A is 0<A≤0.55.

[0054] In some embodiments of the present application, the value range of the first metrological characteristic value A is 0.015≤A≤0.4.

[0055] In some embodiments of the present application, the value range of the first metrological characteristic value A is 0.015≤A≤0.2.

[0056] In some embodiments of the present application, the value range of the second metrological characteristic value B is 0<B≤0.35.

[0057] In some embodiments of the present application, the value range of the second metrological characteristic value B is 0.001≤B≤0.35.

[0058] In some embodiments of the present application, the value range of the second metrological characteristic value B is 0.005≤B≤0.35.

[0059] In some embodiments of the present application, wherein the Li a M b N c R d P e T f O g , 1<a≤6, 0<b<1, 0<c<2, 0<d<3, 0<e<3, 0<f<8, 0<g<12.

[0060] In some embodiments of the present application, the primary particles and / or secondary particles of the powder material are spheroids; the spheroids have a first short axis, a second short axis and a long axis; the long axis is perpendicular to the plane where the first short axis and the second short axis are located; the dimensions of the spheroids at the first short axis, the second short axis and the long axis are x, y, z, respectively, wherein 1≤z / x<2, 1≤z / y<2.

[0061] In some embodiments of the present application, the dimension z of the spheroid on the major axis ranges from 0.01 μm ≤ z ≤ 100 μm.

[0062] In some embodiments of the present application, the dimension x of the spheroid at the first minor axis ranges from 0.01 μm ≤ x ≤ 100 μm.

[0063] In some embodiments of the present application, the dimension y of the spheroid at the second minor axis ranges from 0.01 μm ≤ y ≤ 100 μm.

[0064] In some embodiments of the present application, the dimension z of the spheroid at the major axis is in the range of 0.014μm≤z≤32μm; the dimension x of the spheroid at the first minor axis is in the range of 0.014μm≤x≤32μm; the dimension y of the spheroid at the second minor axis is in the range of 0.014μm≤y≤32μm.

[0065] Optionally, in some embodiments of the present application, the dimension z of the spheroid at the major axis is in the range of 0.014μm≤z≤11μm; the dimension x of the spheroid at the first minor axis is in the range of 0.014μm≤x≤11μm; the dimension y of the spheroid at the second minor axis is in the range of 0.014μm≤y≤11μm.

[0066] Optionally, in some embodiments of the present application, the average particle size of the powder material ranges from 0.1 to 30 μm.

[0067] Optionally, in some embodiments of the present application, the ionic conductivity of the powder material is in the range of 10E -6 -5E -2 S / cm.

[0068] Furthermore, the ionic conductivity of the powder material is in the range of 10E -6 -5E -3 S / cm.

[0069] Reference Figure 4 As shown, the preparation method of the powder material of the present application specifically includes the following steps:

[0070] S101: According to the chemical formula of the powder material Li a M b N c R d P e T f O g Provide the raw materials to be mixed corresponding to each element.

[0071] S102: Mix the multiple raw materials to be mixed provided in step S101 to obtain a precursor material.

[0072] S103: heat-treating the precursor material obtained in step S102 to obtain a heat-treated product.

[0073] S104: crushing, ball milling, drying and sieving the heat-treated product obtained in step S103 to obtain the powder material.

[0074] Wherein, M is selected from at least one of In, Sc, B, Ga, Nb, Y, Zr, Al, Ni, Co, Mn, Mg, Ca, Sr, Cu, Zn, Fe, Na, and K;

[0075] Wherein, N is selected from at least one of Ti, Zr, Hf, Si, Ge, and Sn;

[0076] Wherein, d / (b+c+d+e) is defined as the first metrological characteristic value A; f / (f+g) is defined as the second metrological characteristic value B;

[0077] The value range of the first metrological characteristic value A is 0<A<0.6; the value range of the second metrological characteristic value B is 0<B≤0.4.

[0078] Optionally, in some embodiments of the present application, the raw materials in step S101 may be: Li2CO3, Al2O3, TiO2, SiO2, NH4H2PO4, LiF, wherein LiOH (or Li2CO3) needs to be configured in excess of 15wt% according to the mass calculated by the chemical formula.

[0079] Optionally, in some embodiments of the present application, the specific method of step S102 is:

[0080] The raw materials to be mixed are added to the dispersant in a certain order, and then fully mixed by wet grinding. After the wet grinding and mixing are completed, drying is carried out.

[0081] Wherein, as an optional solution, the dispersant used for wet grinding mixing is selected from one or more of ethanol, propanol, isopropanol, butanol, water, NMP, DMF and acetone.

[0082] Among them, as an optional scheme, specific methods of wet grinding and mixing include but are not limited to ball milling, sand milling, high-speed dispersion, liquid phase spraying, ultrasonic vibration, and electrostatic spinning.

[0083] Among them, as an optional scheme, specific methods of drying treatment include but are not limited to oven drying, belt drying, microwave drying, rotary evaporator, freeze drying, centrifugal drying, and single cone drying.

[0084] Optionally, in some embodiments of the present application, the temperature range of the heat treatment in step S103 is 300-1000°C.

[0085] Optionally, in some embodiments of the present application, the time range of the heat treatment in step S103 is 4-12 hours.

[0086] Optionally, in some embodiments of the present application, the heating rate of the heat treatment in step S103 is in the range of 1-10° C. / min.

[0087] Optionally, in some embodiments of the present application, the equipment used for the crushing process in step S104 includes but is not limited to a jaw crusher, a ball mill, a sand mill, and a gas crusher. As an optional solution, the crushing process can be performed twice or more.

[0088] The present application also provides a method for preparing a positive electrode lithium supplement, which specifically comprises the following steps:

[0089] S201: Mixing the matrix of the positive electrode lithium supplement agent and the powder material for coating.

[0090] S202: sintering the mixed matrix and the powder material.

[0091] Wherein, the matrix is ​​selected from at least one of Li5FeO4, Li2NiO2, and Li6CoO4; the coating layer is formed by a powder material; the powder material can adopt the above-mentioned scheme.

[0092] The present application also provides a lithium battery using the above-mentioned positive electrode lithium replenisher. The above-mentioned positive electrode lithium replenisher is mixed into the positive electrode active material, and the positive electrode lithium replenisher accounts for 0.5% to 2% of the total mass of the positive electrode active material and the positive electrode active material.

[0093] The present application is further described below in conjunction with specific embodiments of the present application.

[0094] Example 1

[0095] 1) Use a 1L high-speed mixer to mix the materials and prepare Li 4.3 Al 0.4 Ti1.6 Si 2.9 P 0.1 F 1.26 O 11.37 The specific preparation of lithium aluminum titanium phosphate solid electrolyte powder includes: the molar ratio of Li, Al, Ti, Si, P, F is 4.3:0.4:1.6:2.9:0.1:1.26, wherein A=0.1, B=0.1. LiOH (or Li2CO3), Al2O3, TiO2, SiO2, NH4H2PO4 and LiF are selected as raw materials, wherein LiOH (or Li2CO3) is in excess of 15wt%, and the precursor powder is fully mixed by a VC mixer. Then, the LATSPF powder is obtained by keeping the temperature at 850°C for 12h, with a heating rate of 3°C / min.

[0096] 2) Use pre-crushing equipment to crush the LATPF powder, add alcohol to prepare a slurry with a certain solid content, and use a ball mill and a sand mill to obtain a 300nm (median particle size D50) level LATSPFO slurry. Then dry the slurry in an oven and finally crush it to obtain the finished LATSPF powder.

[0097] 3) The above-mentioned LATSPF powder and the positive electrode lithium replenisher matrix Li5FeO4 are weighed according to a mass ratio of 0.1:100, and then mixed evenly. In a nitrogen atmosphere, the temperature is kept at 200°C for 10 hours with a heating rate of 3°C / min to obtain a modified lithium battery positive electrode lithium replenisher.

[0098] 4) The above positive electrode lithium replenisher was arranged for XRD and moisture test; after being placed in an air environment with a humidity of 40% for 0h, 1h, and 2h, the lithium replenisher was assembled with Li metal into a Li|positive electrode lithium replenisher button battery. The positive electrode lithium replenisher was mixed with the positive electrode at a ratio of 1% to prepare a positive electrode sheet. The moisture content of the positive electrode sheet was tested, and it was assembled with Li metal into a Li|M90 button battery, and the battery's first cycle efficiency was tested.

[0099] Example 2

[0100] The difference between this embodiment and embodiment 1 is that LATSPF powder and positive electrode lithium supplement agent matrix Li5FeO4 are weighed according to a mass ratio of 5:100, then mixed evenly, and kept at 200°C for 10 hours in a nitrogen atmosphere with a heating rate of 3°C / min.

[0101] The rest of the preparation methods and parameters were the same as those in Example 1.

[0102] Example 3

[0103] The difference between this embodiment and embodiment 1 is that LATSPF powder and positive electrode lithium supplement agent matrix Li5FeO4 are weighed according to a mass ratio of 10:100, then mixed evenly, and kept at 200°C for 10 hours in a nitrogen atmosphere with a heating rate of 3°C / min.

[0104] The rest of the preparation methods and parameters were the same as those in Example 1.

[0105] Example 4

[0106] The difference between this embodiment and embodiment 1 is that LATSPF powder and positive electrode lithium supplement agent matrix Li5FeO4 are weighed according to a mass ratio of 0.1:100, then mixed evenly, and kept at 500°C for 10 hours in a nitrogen atmosphere with a heating rate of 3°C / min.

[0107] The rest of the preparation methods and parameters were the same as those in Example 1.

[0108] Example 5

[0109] The difference between this embodiment and embodiment 1 is that LATSPF powder and positive electrode lithium supplement agent matrix Li5FeO4 are weighed according to a mass ratio of 5:100, then mixed evenly, and kept at 500°C for 10 hours in a nitrogen atmosphere with a heating rate of 3°C / min.

[0110] The rest of the preparation methods and parameters were the same as those in Example 1.

[0111] Example 6

[0112] The difference between this embodiment and embodiment 1 is that LATSPF powder and positive electrode lithium supplement agent matrix Li5FeO4 are weighed according to a mass ratio of 10:100, then mixed evenly, and kept at 500°C for 10 hours in a nitrogen atmosphere with a heating rate of 3°C / min.

[0113] The rest of the preparation methods and parameters were the same as those in Example 1.

[0114] Example 7

[0115] The difference between this embodiment and embodiment 1 is that LATSPF powder and positive electrode lithium supplement agent matrix Li5FeO4 are weighed according to a mass ratio of 0.1:100, then mixed evenly, and kept at 800°C for 10 hours in a nitrogen atmosphere with a heating rate of 3°C / min.

[0116] The rest of the preparation methods and parameters were the same as those in Example 1.

[0117] Example 8

[0118] The difference between this embodiment and embodiment 1 is that LATSPF powder and positive electrode lithium supplement agent matrix Li5FeO4 are weighed according to a mass ratio of 5:100, then mixed evenly, and kept at 800°C for 10 hours in a nitrogen atmosphere with a heating rate of 3°C / min.

[0119] The rest of the preparation methods and parameters were the same as those in Example 1.

[0120] Example 9

[0121] The difference between this embodiment and embodiment 1 is that LATSPF powder and positive electrode lithium supplement agent matrix Li5FeO4 are weighed according to a mass ratio of 10:100, then mixed evenly, and kept at 800°C for 10 hours in a nitrogen atmosphere with a heating rate of 3°C / min.

[0122] The rest of the preparation methods and parameters were the same as those in Example 1.

[0123] Comparative Example 1

[0124] This comparative example provides Li5FeO4 alone as a lithium supplement.

[0125] Comparative Example 2

[0126] Al2O3 powder and positive electrode lithium replenisher matrix Li5FeO4 are weighed in a mass ratio of 0.1:100, then mixed evenly, and kept at 200°C for 10 hours in a nitrogen atmosphere with a heating rate of 3°C / min to obtain a modified lithium battery positive electrode lithium replenisher.

[0127] Comparative Example 3

[0128] Al2O3 powder and positive electrode lithium replenisher matrix Li5FeO4 are weighed in a mass ratio of 10:100, then mixed evenly, and kept at 200°C for 10 hours in a nitrogen atmosphere with a heating rate of 3°C / min to obtain a modified lithium battery positive electrode lithium replenisher.

[0129] Comparative Example 4

[0130] Al2O3 powder and positive electrode lithium replenisher matrix Li5FeO4 are weighed in a mass ratio of 0.1:100, then mixed evenly, and kept at 800°C for 10 hours in a nitrogen atmosphere with a heating rate of 3°C / min to obtain a modified lithium battery positive electrode lithium replenisher.

[0131] Comparative Example 5

[0132] Al2O3 powder and positive electrode lithium replenisher matrix Li5FeO4 are weighed in a mass ratio of 10:100, then mixed evenly, and kept at 800°C for 10 hours in a nitrogen atmosphere with a heating rate of 3°C / min to obtain a modified lithium battery positive electrode lithium replenisher.

[0133] Physical and chemical properties testing

[0134] Moisture detection: GB / T 24533-2019 Karl Fischer modified method. Dry the powder at 200℃ for 24h, then place it in an environment of 25℃ and 60% humidity to detect moisture at different times. Moisture detection is completed in a dry room, and the dew point of the dry room is required to be lower than -35℃.

[0135] Lithium ion conductivity detection: The electrochemical workstation is used to detect the AC impedance of the solid electrolyte sheet, and the lithium ion conductivity is calculated by the formula. The detection frequency is 1000000-0.01Hz, the amplitude is 5mA, and each sample is tested in parallel 3 times. Sample preparation: Take 0.5g of dry LATP powder, press it at 300MPa for 1min under a 15mm diameter mold, keep the sheet thickness 1-2mm, heat treat it at 850℃ for 10h, cool it to room temperature and vacuum seal it for storage, and the density is >90%. The LATP sheet is evenly gold-plated on both sides, and then the AC impedance spectrum is detected on EC-Lab. Select a swagelok mold (the inner wall is made of Teflon insulation material), connect the two ends of the LATP sheet with stainless steel sheets, and set the torque wrench to 5mN. According to the formula δ=l / (RS), l and S are the sheet thickness and surface area, respectively, R is the detected AC impedance value, and δ is the lithium ion conductivity.

[0136] Powder conductivity test: GBT30835-2014 "Carbon composite lithium iron phosphate cathode material for lithium-ion batteries". Four-probe test principle, applied pressure range 10-200MPa, pressurization interval 10MPa, pressure maintenance 10s, pressure relief to 3MPa, pressure maintenance 10s;

[0137] Phase detection: JY / T 0587-2020 General rules for polycrystal X-ray diffraction methods.

[0138] Morphology detection: JY / T 0584-2020 General rules for scanning electron microscopy analysis methods.

[0139] Laser particle size detection: Prepare a 10% solid content aqueous solution, ultrasonicate for 5 minutes, and detect the particle size on Malvern 3000. Select a refractive index of 2.42 and an absorbance of 1. The dispersant is water, and the refractive index of water is 1.33.

[0140] Specific surface area test: GB / T 19587-2017.

[0141] Contact angle detection: The contact angle detector detects the wettability of electrolyte electrode slurry diaphragm and electrode sheet. The contact angle detection uses a contact angle meter to drop electrolyte on the surface of solid electrolyte sheet / diaphragm / positive electrode / negative electrode sheet, measure the distance and height between the two ends of the droplet, and calculate the contact angle. The smaller the contact angle value, the better the lyophilic ability of the diaphragm.

[0142] Compaction density test: GB / T 24533-2019 and GBT30835-2014 "Carbon composite lithium iron phosphate cathode material for lithium-ion batteries"

[0143] Electrochemical performance testing

[0144] Preparation and testing of button battery: GB / T 24533-2019. The ternary materials M90, Super P and PVDF were weighed in a ratio of 96:2:2, dispersed in NMP slurry, and then coated on 16μm thick Al foil and vacuum dried at 100℃ for 12h as the positive electrode. The above-mentioned positive electrode, conventional PP diaphragm and Li metal negative electrode were used to assemble CR232 button batteries, in which the positive and negative electrode diameters were 15mm, the diaphragm diameter was 20mm, and the electrolyte was 1mol / LLiPF6-EC / DEC / EMC battery, and 1C constant current charge and discharge test was performed. The constant current charge and discharge voltage range is 2.5V-4.3V, and the current is 1C.

[0145] Preparation and testing of soft-pack batteries: The ternary materials M94, LMNSPTO, Super P and PVDF were weighed in a ratio of 96:1:1:2 (coating system, M94, Super P and PVDF ratio is 96%:2%:2%), dispersed in NMP slurry, and then coated on 16μm thick Al foil, and vacuum dried at 80℃ for 12h as the positive electrode. Graphite, acetylene black, CMC and SBR were weighed in a ratio of 95:2.5:1.5:1, dispersed into an aqueous slurry, and then coated on a 10μm copper foil, and vacuum dried at 100℃ for 12h as the negative electrode. The above-mentioned positive electrode, conventional PP separator and negative electrode were used to assemble a 2Ah soft-pack battery. The electrolyte was 1.2mol / LLiPF6-EC / DEC / EMC+1.5%VC+1.5%FEC+2.5%PS battery, and 1C constant current charge and discharge test was performed. The constant current charge and discharge voltage range is 2.5V-4.3V, and the current is 1C. For all-solid-state batteries, the positive electrode and the negative electrode are directly hot-pressed at a temperature of 300°C and a pressure of 300MPa-20S, and then encapsulated in an aluminum-plastic film to prepare a 2Ah all-solid-state soft-pack battery. The constant current charge and discharge voltage range is 2.5V-4.3V, and the current is 0.2C.

[0146] Battery safety performance testing:

[0147] High temperature thermal storage retention rate and recovery rate: GB / T 31484-2015. The battery in the fully charged state is fully charged at 1C, stored at 55℃ for 7 days, cooled to 25℃, and left to stand for 4 hours. The capacity retention rate and recovery rate are tested respectively.

[0148] Hot box test: GB / T 36276-2023 "Lithium-ion batteries for power energy storage" Place a 2Ah soft pack battery in a high temperature oven with a protective environment, and perform a 45℃-200℃ program heating process, heating at 5℃ / min, keeping the temperature for 30 minutes every 5℃, and perform hot box safety testing to observe whether the battery catches fire, smokes or explodes. Six parallel samples are required for each group.

[0149] Acupuncture: GB 31241-2014 and GB / T 31485-2015, GB 38031-2020. Select a 2Ah small soft-pack battery, fully charge the battery, and use a high-temperature resistant steel needle with a diameter of 5-8 mm to vertically penetrate the battery plate at a speed of (25±5) mm / s. The steel needle stays in the battery for 1 hour without catching fire or exploding to be qualified. It is required that there are fire-fighting facilities and an open environment around, and the operator has professional ability and protective measures. 8 parallel samples per group.

[0150] The test results are shown in Tables 1 to 3.

[0151] Table 1 shows the first cycle charging specific capacity of the positive electrode lithium supplement agents of different embodiments and comparative examples placed in an air environment for different time periods.

[0152] Table 2 shows the physicochemical performance data of the positive electrode lithium supplement agents of different embodiments and comparative examples.

[0153] Table 3 shows the electrochemical performance test data of button cells formed from powder materials of different embodiments and comparative examples.

[0154] Table 1

[0155]

[0156] Table 2

[0157]

[0158] Table 3

[0159]

[0160] Referring to Tables 1 to 3, the first cycle charge capacity data of different embodiments and comparative examples after being stored for different periods of time in an air atmosphere with a humidity of 40%.

[0161] Since the ionic conductivity is improved in the examples, the first cycle specific capacity of Examples 1-9 is higher than that of Comparative Examples 2-5.

[0162] Due to the hydrophobic spherical LMNSPTO material coated on the surface of the examples, the moisture content of the powders of Examples 1-9 is lower than that of Comparative Examples 1-5.

[0163] The first efficiency of Example 1-9 is improved by about 2% compared with Comparative Example 1-5; this may be attributed to the reverse replenishment of lithium ions in the solid electrolyte coated on the surface of the positive electrode lithium replenisher into the positive electrode lithium replenisher.

[0164] The above is a detailed introduction to the battery, positive electrode lithium supplement and preparation method thereof provided in the embodiments of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method and core idea of ​​the present application. At the same time, for technicians in this field, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A positive electrode lithium supplement, Features: The positive electrode lithium supplement comprises: substrate and cladding; Wherein, the matrix is ​​selected from Li 5 FeO 4 , Li 2 NiO 2 , Li 6 CoO 4 At least one of; Wherein, the coating layer is formed of powder material; The chemical formula of the powder material is Li a M b N c R d P e T f O g ; Wherein, M is selected from at least one of In, Sc, B, Ga, Nb, Y, Zr, Al, Ni, Co, Mn, Mg, Ca, Sr, Cu, Zn, Fe, Na, and K; Wherein, N is selected from at least one of Ti, Zr, Hf, Si, Ge, and Sn; Wherein, R is selected from at least one of Nb, Ti, Zr, Hf, As, Sb, Si, Ge, and Sn, and R and N are selected from different elements respectively; Among them, T is selected from at least one of S, Se, N, F, Cl, Br, and I.

2. The positive electrode lithium supplement according to claim 1, Features: The primary particles and / or secondary particles of the powder material are spheroids; the spheroids have a first short axis, a second short axis and a long axis; the long axis is perpendicular to the plane where the first short axis and the second short axis are located; the dimensions of the spheroids at the first short axis, the second short axis and the long axis are x, y, z, respectively, wherein 1≤z / x<2, 1≤z / y<2.

3. The positive electrode lithium supplement as claimed in claim 2, Features: The dimension z of the spheroid on the major axis ranges from 0.01 μm ≤ z ≤ 100 μm.

4. The positive electrode lithium supplement according to claim 1, characterized in that: in, d / (b+c+d+e) is defined as the first metrological characteristic value A; the value range of the first metrological characteristic value A is 0<A<0.

6.

5. The positive electrode lithium supplement according to claim 4, characterized in that: in, f / (f+g) is defined as a second metrological characteristic value B; the value range of the second metrological characteristic value B is 0<B≤0.

4.

6. The positive electrode lithium supplement according to claim 4, characterized in that: in, The Li a M b N c R d P e T f O g where 1 < a ≤ 6, 0 < b < 1, 0 < c < 2, 0 < d < 3, 0 < e < 3, 0 < f < 8, 0 < g < 12.

7. A method for preparing a positive electrode lithium supplement, Features: Mixing the matrix of the positive electrode lithium supplement agent and the powder material for coating; Sintering the mixed matrix and powder material; Wherein, the matrix is ​​selected from Li 5 FeO 4 , Li 2 NiO 2 , Li 6 CoO 4 At least one of; Wherein, the coating layer is formed of powder material; The chemical formula of the powder material is Li a M b N c R d P e T f O g ; Wherein, M is selected from at least one of In, Sc, B, Ga, Nb, Y, Zr, Al, Ni, Co, Mn, Mg, Ca, Sr, Cu, Zn, Fe, Na, and K; Wherein, N is selected from at least one of Ti, Zr, Hf, Si, Ge, and Sn; Wherein, R is selected from at least one of Nb, Ti, Zr, Hf, As, Sb, Si, Ge, and Sn, and R and N are selected from different elements respectively; Wherein, T is selected from at least one of S, Se, N, F, Cl, Br and I.

8. The preparation method according to claim 7, Features: The sintering temperature for sintering the mixed matrix and the powder material is in the range of 200-800° C., the sintering time is in the range of 3-12 hours, the temperature rise rate is in the range of 1-10° C. / min, and the sintering atmosphere is nitrogen.

9. The preparation method according to claim 7, Features: The mass ratio of the powder material to the matrix is ​​(0.1-10):

100.

10. A battery, Features: The invention comprises the positive electrode lithium supplement agent as claimed in any one of claims 1 to 6; and / or comprises the lithium supplement agent prepared by the preparation method as claimed in any one of claims 7 to 9.

Citation Information

Patent Citations

  • High-nickel long-life multi-element positive electrode material and preparation method thereof

    CN109755512A

  • Positive Electrode Active Material for High Voltage Comprising Lithium Manganese-Based Oxide and Preparation Method Thereof

    CN110383543A

  • Multi-element cathode material, preparation method thereof and lithium ion battery

    CN111162271A

  • Lithium supplement additive and particle size control method and application thereof

    CN115312769A

  • Composite cathode active material, method of preparing the same, and cathode and lithium battery including the composite cathode active material

    US20150228970A1