Recovery of rare earth elements

By dissolving phosphate rock and cooling the carbonate melt to form new rare earth element compounds, the problem of harsh chemical treatment and thorium uranium processing in the existing technology is solved, and the efficient recovery of rare earth elements and the sustainability and economy of resources are achieved.

CN118843705APending Publication Date: 2024-10-25AUSTRALIEN NAT UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024737.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-20
Filing Date
2023-01-20
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing technologies rely on harsh chemical treatments in the recovery of rare earth elements, and present challenges in handling thorium and uranium waste, affecting the sustainability and economics of the resource.

Method used

By using carbonate melt to dissolve phosphate rock, reversing the natural formation process of phosphate rock, releasing and cooling to form new rare earth element compounds, avoiding concentrated acid or concentrated alkali treatment, and doing it under ambient pressure, utilizing carbonate-based Eutectic mixtures of fluxes reduce energy consumption and costs.

Benefits of technology

It achieves efficient recovery of rare earth elements, reduces the extraction of thorium and uranium, reduces energy consumption and costs, and improves the sustainability and economy of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118843705A_ABST
    Figure CN118843705A_ABST
Patent Text Reader

Abstract

Disclosed herein are methods of recovering one or more rare earth elements from phosphorite comprising one or more rare earth elements. The method may include mixing a phosphate ore comprising one or more rare earth elements with a carbonate-based flux. The method may also include subjecting the mixture to conditions such that one or more rare earth elements are released from the phosphorite and one or more rare earth element compounds are formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for recovering rare earth elements from, in particular, phosphate ores, such as monazite, xenotime and apatite. The method uses a molten carbonate-based flux to dissolve the phosphate ore containing the rare earth elements, and then cools the molten mixture, thereby allowing the formation of different rare earth element compounds. The method is also suitable for recovering elements from oxide and silicate minerals, such as niobium and tantalum from oxides, rare earth elements from pyroxene, and zirconium from zircon. Background Art

[0002] Rare earth elements are considered important metals because they are essential in the production of many modern devices, such as mobile phones, magnets and batteries. Rare earth elements are also used as catalysts, in ceramic and glass production, in lasers, as metal alloys, etc.

[0003] Demand for rare earth elements has grown rapidly over the past decade. The supply of rare earth elements is dominated by China, which produced nearly 60% of global rare earth oxide equivalent in 2020. Reliance on one country for a large portion of the world's resources can put supply at risk, for example, in 2010, China restricted its exports of rare earth elements due to geopolitical issues.

[0004] Currently, only three REE-containing minerals are considered economical to mine. They are monazite [(Ce,La,Nd,Th)PO4], cerium fluoride carbonate [(Ce,La,Y)CO3F], and xenotime [YPO4], all of which contain a number of other REEs in place of Y and Ce. Two of these three minerals are phosphates. Apatite [Ca3(PO4)5(F,Cl,OH)] is another phosphate that can also be mined, but contains much lower concentrations of REEs (i.e., no REEs in the molecular formula). Phosphate rock, a sedimentary rock rich in apatite, is another potential source of REEs. The traditional extraction routes for phosphate-based minerals containing REEs are similar.

[0005] The mineral-bearing ore is first subjected to beneficiation to separate and concentrate the minerals containing rare earth elements. Beneficiation may include processes such as flotation, electrostatic force separation, gravity separation or magnetic separation. The separated rare earth element-containing minerals are then pretreated by roasting or digesting the ore at elevated temperatures (200-600°C) in the presence of an acid or base (as a solution or solid). A solution containing the rare earth elements is formed by a combination of methods (which may include water leaching, sodium hydroxide treatment and / or a second acid leaching stage). Contaminating elements are removed from this solution by various methods, and the REEs are then precipitated as oxides or carbonates.

[0006] Critical to the future of the global rare earth element industry is finding new ways to mine and extract rare earth elements from deposits. New methods also need to take into account concerns about thorium and uranium waste, as these radioactive elements are often associated with the minerals that contain them.

[0007] It should be understood that reference to prior art herein does not constitute an admission that the prior art forms part of the common general knowledge in the art, in Australia or any other country. SUMMARY OF THE INVENTION

[0009] In a first aspect, disclosed herein is a method for recovering one or more rare earth elements from a phosphate ore containing one or more rare earth elements. Surprisingly and advantageously, by using a carbonate melt to dissolve the phosphate ore, the method can utilize the mechanism by which the phosphate ore containing rare earth elements is naturally formed from a carbonate melt.

[0010] In nature, many phosphate ores containing rare earth elements crystallize from carbonate melts or carbonate magmas. During their formation, the carbonate melts may have been enriched with rare earth elements. As the carbonate melts cool, various minerals are formed. These minerals may include carbonates, phosphates (such as monazite, apatite, and xenotime), and oxides of other metals (such as pyrochlore).

[0011] Rocks derived from carbonate magma are called carbonatites. Compared with other igneous rocks, carbonate rocks contain relatively high concentrations of rare earth elements (>500ppm) and varying amounts of thorium and uranium. Although carbonate magma is much rarer than silicate magma, there are still more than 500 known carbonate rocks in the world.

[0012] Since naturally occurring natural phosphate minerals containing rare earth elements can be formed (crystallized) from carbonate melts, by subjecting the phosphate minerals (e.g., monazite, xenotime, apatite, phosphorite) to molten carbonates, the phosphate minerals can be decomposed (or redissolved), thereby releasing the rare earth elements from the mineral structure. During cooling, the rare earth elements can partition into the carbonate phase.

[0013] Naturally occurring natural phosphate ores containing rare earth elements may also be in the form of sedimentary rocks, such as phosphorite. Although the natural mechanism of formation is different from that of igneous phosphate ores (i.e., through the deposition and compaction of sediments rather than volcanic activity), sedimentary phosphate ores may still be decomposed (or dissolved) by carbonate melts.

[0014] Thus, the methods disclosed herein may include mixing a phosphate rock comprising one or more rare earth elements with a carbonate-based flux.Both the carbonate-based flux and the phosphate rock are typically in the form of finely divided solids.

[0015] The method may also include subjecting the mixture to conditions such that one or more rare earth elements are released from the phosphate ore and form one or more (new) rare earth element compounds upon cooling. The one or more rare earth element compounds formed upon cooling are different from the one or more rare earth element minerals present in the phosphate ore. The newly formed rare earth element compounds are soluble in acid. Without wishing to be bound by theory, the inventors speculate that the new rare earth element compounds are rare earth element carbonate and / or oxide compounds.

[0016] A major advantage of the method disclosed herein is that it does not rely on harsh chemical treatments to break down the structure of the phosphate rock, such as concentrated acids or alkalis. Instead, the natural process of phosphate rock formation is actually reversed by adding the phosphate rock to a carbonate melt.

[0017] In some embodiments, the conditions to which the mixture is subjected may include subjecting the mixture to a temperature that melts the carbonate-based flux. The mixture may be maintained at the temperature for a predetermined time. The phosphate ore containing one or more rare earth elements may be substantially dissolved in the molten carbonate-based flux. As the phosphate ore dissolves, the one or more rare earth elements may be released therefrom.

[0018] In some embodiments, the conditions to which the mixture is subjected may also include solidifying the molten mixture after a predetermined time has passed. Along with the solidification of the molten mixture, one or more new rare earth element (may be carbonate and / or oxide) compounds can thereby form a solid. Solidification rate is usually fast enough to ensure that the rare earth element is combined with the new (may be carbonate and / or oxide) rather than combined with phosphate. On a smaller scale, the molten mixture is allowed to solidify, for example, by no longer subjecting the mixture to heating, the cooling rate can be made fast enough, so that the rare earth element forms carbonate and / or oxide minerals. However, on a larger scale (for example, using a larger mass of phosphate rock and carbonate-based flux), the larger thermal mass of the larger mixture may cause the cooling rate to be slower. Therefore, in order to maximize the recovery rate of the rare earth element, solidification may therefore also include rapidly solidifying the molten mixture. For example, the mixture can be rapidly cooled using air or water.

[0019] In some embodiments, the elevated temperature may be in the range of about 500°C to about 650°C. The elevated temperature is typically about 50°C higher than the melting point of the carbonate-based flux. In this regard, the melting point of the carbonate-based flux depends on the composition of the flux. For example, in other embodiments where the melting point of the carbonate-based flux is higher, the elevated temperature may be as high as about 800°C. In other embodiments, the carbonate-based flux may be heated to more than 50°C above its melting point. For example, to promote the reaction between the flux and the mineral.

[0020] In some embodiments, the predetermined time can be about 2 hours. The predetermined time should be enough to ensure that the carbonate-based flux is melted, and the phosphate ore containing one or more rare earth elements is substantially dissolved. However, the predetermined time can be controlled not to be too long, otherwise melting may cause partial decarburization of the carbonate-based flux, thereby reducing the recovery rate of the rare earth element. Flux decarburization also reduces the amount of recyclable and recyclable flux, thereby affecting the economic feasibility of the method.

[0021] In some embodiments, the method can be carried out at ambient pressure. However, pressure can depend on the type of selected carbonate-based flux. For example, when using sodium carbonate and / or potassium carbonate-based flux, the method can be carried out at ambient pressure. On the other hand, if calcium carbonate and / or magnesium carbonate-based flux are used, the conditions to which the mixture is subjected can include elevated pressure. This is because elevated pressure is required to minimize the degree of decarburization (e.g., using calcium carbonate and / or magnesium carbonate-based flux). Therefore, sodium carbonate and / or potassium carbonate-based flux are preferably used, because the method can be carried out at ambient pressure. In addition, the elevated pressure required for minimizing calcium carbonate and / or magnesium carbonate-based flux decarburization is often very uneconomical.

[0022] Phosphate ores containing one or more rare earth elements may also contain uranium and / or thorium, both of which are radioactive. The methods disclosed herein may be advantageously performed compared to prior methods because by changing the conditions to which the carbonate-based flux and the phosphate ores are subjected, the extraction of uranium and / or thorium may be reduced.

[0023] In some embodiments, the residue of the one or more rare earth element compounds and solids obtained can be separated. For example, separation of the new rare earth element compound and the residue of the solid can include crushing the solid containing the one or more new rare earth element compounds, thereby producing a crushed solid. The solid can be crushed to increase the surface area to volume ratio, which can increase the speed at which the subsequent stages of the method occur. Typically, the solid is crushed into a fine powder.

[0024] In some embodiments, separation of the new rare earth element compound from the solid residue may also include washing the crushed solid with water to substantially dissolve the residual carbonate-based flux therefrom. In this regard, the wash water containing the dissolved residual carbonate-based flux may be separated. For example, filtration may be utilized to achieve such separation. The separated wash water may be further processed to recover the carbonate-based flux in a solid form substantially free of liquid. For example, such further processing may include evaporation.

[0025] In some embodiments, a solid carbonate-based flux that is substantially free of liquid may be recycled to constitute at least a portion of the carbonate-based flux. It will therefore be appreciated that another advantage of the methods disclosed herein is that the primary reagent (i.e., carbonate-based flux) may be recovered and recycled, thereby reducing the amount of fresh flux required. This may improve the economic viability of the method.

[0026] In some embodiments, the residue of separating the new rare earth element compound and the mixture also includes the poor co-solvent crushing solid obtained by washing with acid, to dissolve one or more new rare earth element compounds substantially therefrom. Thus, a solution and residue containing one or more rare earth elements can be produced. For example, the concentration of the washing acid can be about 1M. It should be appreciated that the concentration of the washing acid should depend on the type of acid used. For example, for strong acids (such as mineral acids), a concentration of 1M can be sufficient.

[0027] In some embodiments, the washing acid may include a mineral acid. For example, the mineral acid may include one of nitric acid, hydrochloric acid, or sulfuric acid.

[0028] In some embodiments, separation of the new rare earth element compound from the solid residue may also include separation of a solution containing one or more rare earth elements from the residue. For example, the separation may be performed by filtration. Optionally, the solution containing one or more rare earth elements may be further processed to remove impurity elements (e.g., U, Th, Ra, and / or Fe) and produce one or more rare earth element products.

[0029] In some embodiments, a mixture comprising a phosphate ore comprising one or more rare earth elements and a molten carbonate-based flux may include a greater proportion of carbonate-based flux by mass than the phosphate ore comprising one or more rare earth elements. For example, the ratio of carbonate-based flux to phosphate ore by mass may be at least 2: 1. The amount of carbonate-based flux may be sufficient to almost completely dissolve the phosphate ore, thereby maximizing the recovery of the rare earth elements.

[0030] In some embodiments, the phosphate rock may include at least one of the minerals monazite, xenotime or apatite. It should be appreciated that when the mineral comprising one or more rare earth elements is a phosphate mineral, the method disclosed herein becomes applicable. It should be further appreciated that the method may be used to recover rare earth elements from minerals other than monazite, xenotime and apatite. For example, the method may be used to recover rare earth elements from sedimentary rocks (e.g., phosphorite).

[0031] In some embodiments, carbonate-based fluxes may include sodium carbonate and potassium carbonate. Sodium carbonate and potassium carbonate-based fluxes may be synthetic. It should be appreciated that in nature, most known carbonate rock deposits (i.e., natural carbonates) are primarily composed of calcium carbonate and magnesium carbonate. However, when heated at normal pressure, they decarbonize (decompose to release CO2) rather than melt. The reason why calcium carbonate and magnesium carbonate exist in nature is that they are formed and cooled deep in the earth, and therefore are subject to pressure. On the other hand, carbonates primarily composed of sodium and potassium melt under atmospheric pressure before decarbonization. Compared with magnesium carbonate / calcium carbonate melts, sodium carbonate and potassium carbonate melts also have lower melting points. For example, a volcano (Oldoinyo Lengai in Tanzania) is currently erupting sodium-potassium (plus some calcium) carbonate magma, which is stable under atmospheric pressure. The Lengai mixture also contains other elements (including strontium, barium, silicon, and iron) that combine to provide carbonate melts with melting points below about 600°C.

[0032] In some embodiments, sodium carbonate and potassium carbonate fluxes may also include chloride. Chloride may be present in the form of at least one of sodium chloride or potassium chloride. Adding chloride may reduce the fusing point of carbonate-based fluxes. Since the method is usually carried out at a temperature higher than the fusing point of carbonate-based fluxes (i.e., so it melts), by reducing the fusing point of the flux, the total energy requirement may also be reduced.

[0033] In some embodiments, the carbonate-based flux may include about 30% sodium carbonate, about 50% potassium carbonate, and about 20% potassium chloride. In other words, a eutectic mixture of sodium carbonate, potassium carbonate, and potassium chloride. Such carbonate-based flux may be synthetic.

[0034] In other embodiments, carbonate-based fluxes may instead comprise sodium carbonate and sodium chloride. Such carbonate-based fluxes may be synthetic. It should be appreciated that natural carbonate melts may comprise large amounts of potassium carbonate. Although potassium carbonate is a relatively inexpensive reagent, it may be much more expensive than sodium carbonate or sodium chloride. Therefore, fluxes comprising sodium carbonate and sodium chloride may provide significant economic advantages compared to fluxes comprising potassium-based reagents.

[0035] In some of these other embodiments, the carbonate-based co-solvent may comprise, by weight, about 60% sodium carbonate and about 40% sodium chloride. In other words, a eutectic mixture of sodium carbonate and sodium chloride.

[0036] In this regard, it should be appreciated that different compositions of sodium carbonate and / or potassium carbonate and / or sodium chloride and / or potassium chloride can be used as carbonate-based fluxes in the methods disclosed herein, albeit with different melting points. In particular, the flux may comprise any combination of sodium carbonate and / or potassium carbonate and / or sodium chloride and / or potassium chloride.

[0037] In some embodiments, when one or more rare earth elements are released from phosphate ore, the phosphate in the phosphate ore can be converted into sodium phosphate (e.g., trisodium phosphate) and / or potassium phosphate. In particular, the phosphate in the phosphate ore can be dissolved in a molten carbonate-based flux. As the resulting melt cools, the phosphate can form sodium phosphate and / or potassium phosphate. For example, when the cosolvent comprises sodium, the phosphate can be converted into sodium phosphate. For another example, when the cosolvent comprises potassium, the phosphate can be converted into potassium phosphate. For another example, when the cosolvent comprises sodium and potassium simultaneously, the phosphate can be converted into sodium phosphate and potassium phosphate. The sodium phosphate and / or potassium phosphate formed in this way can be dissolved when the solid residue is washed with water, thereby substantially dissolving the residual carbonate cosolvent therefrom. In this regard, the washing water containing the dissolved residual carbonate-based cosolvent can also contain sodium phosphate and / or potassium phosphate.

[0038] In some embodiments of these embodiments, the method may further include separating the sodium phosphate and / or potassium phosphate from the carbonate-based flux. For example, the sodium phosphate and / or potassium phosphate may be separated by fractional crystallization during solution evaporation. The recovered sodium phosphate and / or potassium phosphate may represent a valuable byproduct of the method.

[0039] In some embodiments, carbonate-based fluxing agents may also include other elements added in small amounts. For example, sodium carbonate and potassium carbonate (and / or sodium chloride and potassium chloride) fluxing agents may include lithium chloride or calcium chloride or strontium chloride or barium chloride added in small amounts and / or lithium carbonate or calcium carbonate or strontium carbonate or barium carbonate in the form of lithium or calcium or strontium or barium. Another example is that sodium carbonate and sodium chloride fluxing agents may include lithium chloride or calcium chloride or strontium chloride or barium chloride added in small amounts and / or lithium carbonate or calcium carbonate or strontium carbonate or barium carbonate. Other elements added in small amounts may be selected to reduce the melting point of fluxing agents. With the further addition of more (impurity) elements, the melting point may be further reduced. However, adding more (impurity) elements may increase the complexity of manufacturing and recycling fluxing agents. Since more raw materials may be needed, the cost may also increase. It should be appreciated that it is preferred to select fluxing agents with as few elements as possible to minimize the complexity of the cost and method.

[0040] In some embodiments, the ore containing one or more rare earth elements may be pretreated. For example, bulk ore containing one or more rare earth elements may be pretreated by utilizing flotation or gravity separation. The pretreated ore may then be mixed with a carbonate-based flux.

[0041] An application of the methods disclosed herein may be for extracting rare earth elements from monazite "waste" produced as a byproduct of titanium production from beach sands. Monazite is present in many beach sands. When titanium is mined from beach sands, the monazite is removed and discarded. Currently, this represents "waste" that must be disposed of. However, using the methods disclosed herein, the monazite can be processed to recover the rare earth elements therein. Additionally or alternatively, the monazite in the beach sand can be mined directly.

[0042] Another application of the method disclosed herein may be for treating residual mine tailings. When phosphate minerals are mixed with other minerals, the rock needs to be crushed so that the phosphate minerals are usable. For example, the phosphate minerals can be optionally separated and concentrated by froth flotation. The crushing stage requires a lot of energy consumption, and crushing accounts for about 56% of the total energy consumption in the mining industry. After the ore is crushed, the residual tailings may be rich in rare earth elements as part of another processing operation such as copper or gold recovery. The crushing costs have already been incurred, and if the residual tailings are further processed to concentrate the phosphates for the method of the present invention, more value can be obtained from the waste.

[0043] In a second aspect, the present invention also discloses a method for recovering a metal or metals from an oxide ore containing the metal or metals. The method of the second aspect may be applicable to treating certain oxides, such as but not limited to pyrochlore, columbite, niobium ore or tantalite, i.e., where carbonate melts may have formed natural oxides. However, the method of the second aspect may not be applicable to other metal oxides, i.e., where the oxides may not be formed by carbonate melts or may not be soluble in carbonate melts.

[0044] The method of the second aspect may comprise mixing an ore comprising an oxide of a metal or metals with a carbonate-based flux.

[0045] The method of the second aspect may further comprise subjecting the mixture to conditions such that the metal or metals are released from the oxide ore and one or more carbonate or oxide minerals comprising the metal or metals are formed.

[0046] In some embodiments, the method of the second aspect may also include separating one or more metal carbonate or oxide minerals from the residue of the mixture. For example, the oxide ore mineral may include at least one of the minerals pyrochlore, columbite, niobium ore or tantalite, and the metal or metals may include at least one of the metals niobium or tantalum. However, it should be appreciated that the method of the second aspect is not limited to minerals containing niobium or tantalum.

[0047] In some embodiments, the method of the second aspect may be otherwise identical to the method of the first aspect.

[0048] In some embodiments, the carbonate-based flux may also contain one or more of chlorides, silica, phosphates. It is believed that the addition of silica and / or phosphates may aid in the dissolution of oxide ores in the carbonate-based flux.

[0049] In a third aspect, the present invention also discloses a method for recovering a certain metal or certain metals from a silicate ore containing the certain metal or certain metals. The method of the third aspect can be suitable for processing certain silicates, such as zircon (to extract zircon), pyroxene (to extract rare earth elements) and spodumene (to extract lithium).

[0050] The method of the third aspect may comprise mixing a silicate ore comprising a metal or metals with a carbonate-based flux.

[0051] The method of the third aspect may further comprise subjecting the mixture to conditions whereby the metal or metals are released from the silicate ore and one or more carbonate or oxide minerals comprising the metal or metals are formed.

[0052] In some embodiments, the method of the third aspect may further comprise separating the one or more metal carbonate or oxide minerals from the remainder of the mixture.

[0053] In some embodiments of the method of the third aspect, the silicate ore mineral may include at least one of the minerals zircon, spodumene and spodumene, and the metal or metals may include at least one of zircon, at least one rare earth element or lithium.

[0054] In some embodiments, the method of the third aspect may be the same as the method of the first aspect in other respects.

[0055] In some embodiments, the carbonate-based flux may further include one or more of chloride, silica, phosphate. Typically, the carbonate-based flux also includes at least chloride.

[0056] BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Embodiments of the invention will now be described, by way of example only, with reference to the accompanying drawings, in which:

[0058] Figure 1 is a schematic block flow diagram of a method for recovering one or more rare earth elements from a phosphate ore containing the one or more rare earth elements disclosed herein; Figure 1A yes Figure 1 Schematic block flow diagram of an embodiment of the co-solvent and phosphate recovery stages of the process.

[0059] Figure 2 is a graph showing the concentrations (in parts per million) of rare earth elements in the synthetic monazite, natural monazite, and natural xenotime samples used in the Examples herein.

[0060] Figure 3 This is a backscattered electron image of a synthetic monazite sample containing a mixture of monazite and CeO2. The black areas in the image correspond to the voids (porosity) in the sample.

[0061] Figure 4 and Figure 5 is a graph showing the recovery (yield percentage) of rare earth elements from synthetic monazite samples as a function of the ratio of monazite to carbonate-based flux for two different carbonate-based flux compositions (eutectic Na2CO3-K2CO3-KCl compositions, Figure 4 ; and synthetic analogs of the carbonate melts of Lengai, Figure 5 , see Table 2).

[0062] Figure 6 The XRD spectrum of the residue obtained after reacting synthetic monazite with a carbonate-based flux and recovering the rare earth elements using the method disclosed herein. The marked peak corresponds to CeO2.

[0063] Figure 7 is a graph showing the recovery of rare earth elements from synthetic monazite as a function of time using a eutectic Na2CO3-K2CO3-KCl carbonate-based co-solvent.

[0064] Figure 8 is a graph showing the recovery of rare earth elements U and Th from natural monazite as a function of the ratio of monazite to eutectic Na2CO3-K2CO3-KCl carbonate-based co-solvent. Data for low concentrations (<~1000ppm) of elements in natural monazite are not shown.

[0065] Fig. 9 and Fig.10 is a graph showing the recovery of rare earth elements U and Th from xenotime samples as a function of the ratio of xenotime to carbonate-based co-solvent for two different carbonate-based co-solvent compositions (eutectic Na2CO3-K2CO3-KCl compositions, Fig. 9 ; and synthetic analogs of the carbonate melts of Lengai, Fig.10 , see Table 2). Data for low concentrations (<~1000 ppm) of elements in xenotime are not shown. The low yield of Gd (relative to Sm and Tb) is believed to be an analytical artifact.

[0066] Fig.11is an SEM image of a sample obtained by mixing zircon with a eutectic Na2CO3-NaCl carbonate-based flux and subjecting the mixture to a heat treatment stage.

[0067] Fig.12 is a SEM image of the residue obtained by leaching with water Fig.11 The samples were then calcined at 800 °C. DETAILED DESCRIPTION OF THE INVENTION

[0069] In the following detailed description, reference is made to the accompanying drawings, which form a part of the detailed description. The illustrative embodiments described in the detailed description, depicted in the drawings, and defined in the claims are not intended to be limiting. Other embodiments may be used, and other changes may be made, without departing from the spirit or scope of the subject matter presented. It should be readily understood that the various aspects of the present disclosure, as generally described herein and shown in the drawings, may be arranged, substituted, combined, separated, and designed in a wider variety of different configurations, all of which are contemplated by the present disclosure.

[0070] Disclosed herein is a method for recovering one or more rare earth elements from a phosphate ore containing the one or more rare earth elements. Specific embodiments of the method require only moderately elevated temperatures and readily available reagents, and do not require the use of concentrated acids or bases. More specifically, the phosphate ore containing the rare earth elements is dissolved in a carbonate-based flux at a temperature above the melting point of the carbonate-based flux. The disclosed method effectively "reverse engineers" some of the natural processes by which phosphate ore is formed. In addition, by converting the rare earth elements into different (most likely carbonate and / or oxide) minerals, it is easier to separate the rare earth elements from the residual materials because they are soluble in dilute acid.

[0071] The applicability of the method disclosed herein for recovering one or more rare earth elements from a phosphate ore containing one or more rare earth elements is also illustrated below by way of examples. The examples show that rare earth elements were recovered from a phosphate ore that was mixed with different carbonate-based fluxes in different ratios and maintained at elevated temperatures for different periods of time. The inventors note that the monazite used in Examples 3 and 4 is not pure (as it consists of a mixture of monazite and cerium (IV) oxide). This material somewhat obscures the elegance, simplicity and effectiveness of the method, which would be apparent by using a purer starting material, such as naturally occurring monazite. Example 5 demonstrates the effectiveness of the method for recovering rare earth elements from naturally occurring monazite.

[0072] Now please refer to Figure 1, a conceptual flow chart presented in the form of a simple block diagram illustrates a method 10 for recovering one or more rare earth elements from a phosphate ore containing the one or more rare earth elements. The feed to the method 10 is a phosphate ore 24 containing the one or more rare earth elements.

[0073] Prior to subjecting the ore to process 10, the bulk ore containing phosphate minerals and other minerals containing rare earth elements may be passed through an optional beneficiation stage. In the beneficiation stage, the phosphate minerals containing rare earth elements are pretreated. The bulk ore is subjected to a treatment whereby the phosphate minerals are separated from the other minerals and gangue materials. The treatment includes a series of crushing and separation stages, such as flotation or gravity separation. It should be appreciated that the pretreatment may be tailored to the characteristics of the bulk ore and the phosphate minerals. Known pretreatment methods may be employed. The pretreated phosphate ore is then used as a feed to process 10. Alternatively, the bulk ore may be fed directly to process 10.

[0074] The method 10 comprises a first mixing stage 20, wherein a carbonate-based flux 22 and a phosphate rock containing rare earth elements 24 are mixed in a platinum crucible. Other examples of industrial scale-up are set forth below.

[0075] Both the carbonate-based flux 22 and the phosphate rock 24 are typically in the form of finely divided solids. The mixing stage 20 is performed manually, for example using a mortar and pestle, or by mixing the contents of a platinum crucible with a rod or spoon. The phosphate rock 24 may be pre-treated phosphate rock or crushed (phosphate) ore.

[0076] On an industrial scale, such use of a platinum crucible is not economical. On an industrial scale, the carbonate-based flux 22 and the phosphate rock 24 may be mechanically mixed instead. The inventors speculate that mechanical mixing may include pouring the carbonate-based flux 22 and the phosphate rock 24 from different containers (e.g., hoppers) into a common container at an appropriate rate to achieve the desired flux-to-ore ratio. When the carbonate-based flux 22 and the phosphate rock 24 are poured, they are mixed together. Alternatively, the phosphate rock 24 may be poured directly into the heated carbonate-based flux 22. The heated carbonate-based flux 22 may be in the form of a molten carbonate-based flux.

[0077] The mass of carbonate-based flux 22 added to the platinum crucible is greater than the mass of phosphate rock 24 containing rare earth elements. This is to ensure that there is enough carbonate-based flux 22 to dissolve the phosphate rock 24. The mass ratio of carbonate-based flux 22 to phosphate rock 24 is preferably at least 2:1. A ratio of 2.5:1 extracts at least 50% of the rare earth elements. Reference Figure 4 , Figure 5 and Figures 8 to 10, the effect of mass ratio on rare earth recovery is further illustrated in Examples 3, 5 and 7. The inventors point out that the starting monazite used in Examples 3 and 4 is not pure, and the XRD spectrum reveals the presence of cerium oxide (CeO2) phase in the monazite phase. This material will to some extent obscure the elegance, simplicity and effectiveness of the method, which will be revealed by using a purer starting material. However, reference Figure 8 , Example 5 demonstrates the effectiveness of this method for recovering rare earth elements from naturally occurring monazite.

[0078] Phosphate rock 24 may include phosphate minerals that carry one or more rare earth elements. The mineral may include monazite [(Ce, La, Nd, Th)PO4], xenotime [YPO4], or apatite [Ca3(PO4)5(F, Cl, OH)]. It should be recognized that monazite and xenotime are more economically important than apatite because they contain greater amounts of rare earth elements - apatite does not have any rare earths in its chemical formula. It should also be recognized that many rare earth elements can replace Ce and / or Y in the chemical structure. Thus, these minerals may contain a full set of rare earth elements: La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu plus Y.

[0079] The carbonate-based flux 22 is preferably a sodium carbonate and / or potassium carbonate-based flux. This is because the sodium carbonate / potassium carbonate flux will melt before decomposing at ambient pressure. This allows the next stage of the process, the heat treatment stage 30, to be carried out at ambient pressure. The melting point of a mixture of sodium carbonate and potassium carbonate is also lower than that of a mixture of magnesium carbonate and calcium carbonate.

[0080] Typically, the carbonate-based flux 22 also includes a chloride in the form of sodium chloride and / or potassium chloride. The role of the chloride is to lower the melting point of the carbonate-based flux, thereby reducing the temperature at which the heat treatment stage 30 is performed. A particularly suitable flux comprises about 30% sodium chloride, about 50% potassium carbonate, and about 20% potassium chloride, which will be further described in Examples 3-5 and Example 7 below. The melting point of this composition is 575°C. By adding other elements, the melting point can be further reduced, but care should be taken not to add too many additional elements. Without wishing to be bound by theory, other elements that may be added include lithium (e.g., lithium chloride and / or lithium carbonate) or chlorides and / or carbonates of other elements.

[0081] Another particularly suitable flux comprises about 60% sodium carbonate and about 40% sodium chloride by weight (i.e., a sodium carbonate-sodium chloride eutectic composition), which is further described in the Examples below. This flux composition is particularly advantageous because the cost of sodium carbonate and sodium chloride is much lower than the cost of potassium carbonate. Therefore, the use of this sodium carbonate-based flux can reduce the overall cost of the process. The melting point of this composition is about 632°C. Again, the melting point can be further reduced by adding other elements, but care should be taken not to add too many additional elements. For example, other elements that may be added include chlorides and / or carbonates of lithium (e.g., lithium chloride and / or lithium carbonate) or other elements such as calcium or strontium or barium.

[0082] Alternatively or additionally, the carbonate-based flux 22 also comprises a fluoride, typically in the form of sodium fluoride and / or potassium fluoride. The presence of fluoride in the carbonate-based flux serves to reduce the melting point of the carbonate-based flux, thereby reducing the temperature at which the heat treatment stage 30 is performed. Without wishing to be bound by theory, the inventors speculate that the carbonate-based flux 22 that additionally comprises one or more fluorides may exhibit a lower melting point. For example, it has been observed that the melting point of a carbonate-based flux without chloride but with the addition of fluoride is lower. Such a flux may comprise sodium carbonate and sodium fluoride. As another example, a carbonate flux that contains chloride and with the addition of fluoride has a lower melting point.

[0083] Next, the mixture 26 of carbonate-based flux and phosphate rock is subjected to the heat treatment stage 30 of the method 10. Figure 1 In the method, a platinum crucible containing a mixture of phosphate ore 24 and carbonate-based flux 22 is introduced and heat treated. The heat treatment stage 30 is operated so that substantially all of the rare earth elements are released from the phosphate ore and form new rare earth element compounds upon cooling. The new rare earth element compounds are soluble in acid. Without wishing to be bound by theory, the inventors speculate that the new rare earth element compounds consist primarily of carbonate and / or oxide compounds. This is because it is known that rare earth element carbonates and rare earth element oxides are soluble in acid.

[0084] The heat treatment stage 30 includes a furnace. During the heating step of the heat treatment, the mixture 26 is heated and maintained at a temperature above the melting point of the carbonate-based co-solvent, typically about 500-650° C. The temperature of the furnace is selected to be about 50° C. higher than the melting point of the carbonate-based co-solvent, which depends on the composition of the co-solvent. In this regard, the heating step can include a temperature of up to about 800° C., for example when the melting point of the carbonate-based co-solvent is about 750° C.

[0085] As described above, the heating step may require a temperature of about 800°C or higher. For example, to promote the reaction between the flux and the mineral. The mixture 26 is heated by placing the platinum crucible in a furnace. Typically, the furnace takes the form of a box furnace operating at ambient pressure. At the elevated temperature, the carbonate-based flux melts, thereby producing molten carbonate-based flux. The mixture 26 in the platinum crucible is maintained in the furnace at the elevated temperature for a set time.

[0086] When the mixture 26 is maintained at an elevated temperature, the phosphate ore containing rare earth elements dissolves in the molten carbonate-based flux. The dissolution releases the rare earth elements from the phosphate mineral structure. Upon cooling, the rare earth elements partition into the carbonate phase and form new rare earth element compounds, most likely carbonate and / or oxide compounds. The inventors point out that this is actually a reversal of how the phosphate ore containing rare earth elements was originally formed.

[0087] The predetermined time of heating is sufficient to substantially dissolve the phosphate rock. This allows for almost complete recovery of the rare earth elements from the phosphate rock structure. However, if the predetermined time is too long, the carbonate-based flux will begin to decarburize, thereby reducing the recovery of the rare earth elements and the recovery of the flux. Figure 7 This effect is described more fully in To balance these trade-offs, the effective scheduled time in the furnace is about 2 hours.

[0088] A platinum crucible is a suitable container for mixing 20 and heat treating 30 in a laboratory environment. It will be appreciated that as the process scales up, alternative containers will be needed. Without wishing to be bound by theory, the inventors anticipate that a steel furnace lined with refractory insulation and barrier materials, similar to those used for aluminum processing, would be suitable for carrying out the disclosed process on an industrial scale. Such a container would also replace the need for a box furnace because the contents of the container are heated directly or indirectly in situ. Likewise, industrial-scale containers are typically operated at ambient pressure.

[0089] After a predetermined time has elapsed, the mixture is allowed to cool and solidify in the platinum crucible, thereby producing a cooled solid 32. Cooling is achieved simply by turning off the heating elements of the furnace and allowing the mixture of dissolved phosphate ore and molten carbonate-based flux to cool within the furnace as the furnace cools. The cooled solid 32 contains new rare earth element compounds and residual phosphate minerals, as well as residual (unreacted) solid carbonate-based flux material.

[0090] Cooling is generally rapid enough to ensure that the rare earth elements form new (acid soluble) rare earth element compounds and do not recrystallize into phosphate minerals. Cooling seeks to avoid the natural formation of phosphate rocks containing rare earth elements (i.e., rare earth element phosphate minerals crystallize out of the melt when carbonate rocks are slowly cooled). As described in detail in the examples, cooling the mixture in a furnace with the heating elements turned off produces a cooling rate rapid enough to ensure the formation of acid soluble rare earth element (i.e., presumably carbonate and / or oxide) minerals.

[0091] The cooled solid 32 is subjected to an optional crushing stage 40. The purpose of the crushing stage 40 is to produce fine particles for subsequent processing stages. Crushing ensures that the remaining carbonate-based flux is available for the water washing stage 50 and that the new rare earth element compound is available for the acid washing stage 60.

[0092] Crushing is usually used because the mixture of dissolved phosphate rock and molten carbonate-based flux will agglomerate when cooled, thereby forming large particles. In the agglomerate, not all new rare earth element compounds can be directly obtained because they may be combined in other phases. Typically, the cooled solid 32 will be in the form of a large number of small, tightly connected crystals. On a laboratory scale, the crushing stage 40 includes grinding the solid using a mortar and pestle until uniform fine particles are formed. On an industrial scale, the crushing stage 40 may include a mill, such as a ball mill. Since the cooled solid 32 is brittle, only slight crushing of the cooled solid 32 is required. For example, the energy required to crush the cooled solid 32 is only a small fraction of the energy required to crush the ore in a pre-treatment stage, etc. The crushed solid 42 is delivered to a water washing stage 50.

[0093] In the water washing stage 50, the crushed solids 42 are washed with water 52. The water 52 used to wash 50 the crushed solids 42 can be recycled process water or fresh water. The water washing stage 50 can be carried out batchwise or continuously. For example, the crushed solids and water can be kept in a container for a set time while the container is subjected to agitation to promote mixing therein (i.e., batch processing). Alternatively, the crushed solids and water can be passed through several containers in series (e.g., a continuous stirred tank reactor - i.e., a continuous process).

[0094] Since the residual carbonate-based flux present in the crushed solid 42 is highly soluble in water, by washing the crushed solid 52 with water, the residual carbonate-based flux is substantially dissolved in the water, thereby forming a solution 54 containing the carbonate-based flux. Any soluble impurities (e.g., salts) in the water 52 used for washing 50 will also be contained in the solution 54 containing the carbonate-based flux. The source of the washing water 52 can be determined in advance. For example, if the recycled process water is pure enough, it can be used as the washing water 52. Under these conditions, the water washing stage 50 dissolves only negligible rare earth element compounds.

[0095] When the flux 22 comprises sodium and / or potassium (i.e. sodium carbonate, sodium chloride, potassium carbonate and / or potassium chloride), the solution 54 comprising the carbonate-based flux also comprises phosphates which, when evaporated, will produce sodium phosphate, possibly trisodium phosphate and / or potassium phosphate. This is because, when the flux 22 comprises sodium carbonate and / or potassium carbonate, some or all of the phosphates in the ore 24 are converted into sodium phosphate and / or potassium phosphate. In particular, during heat treatment, the phosphates in the phosphate ore will dissolve in the carbonate-based flux. During cooling, the phosphates thus form sodium phosphate and / or potassium phosphate. The resulting sodium phosphate and / or potassium phosphate are soluble in water and are dissolved in the wash water 52 during washing 50. In this regard, the solution 54 comprises sodium phosphate and / or potassium phosphate and a carbonate-based flux.

[0096] The solution 54 and remaining solids 56 are separated, for example using filtration or by decantation. Typically, the separated solution 54 is recycled for further processing in the flux and phosphate recovery stage 60 to recover the carbonate-based flux 62 in solid form substantially free of liquid.

[0097] In the flux and phosphate recovery stage 60, sodium and / or potassium phosphate 57 and carbonate-based flux 62 are recovered from the solution 54 as separate products. Figure 1A An embodiment of a flux and phosphate recovery stage 60 is shown in which fractional crystallization is used to separate sodium phosphate and / or potassium phosphate and carbonate-based flux. In the illustrated embodiment, the flux and phosphate recovery stage 60 uses fractional crystallization to recover carbonate-based flux and sodium phosphate and / or potassium phosphate from solution 54. In particular, the flux and phosphate recovery stage 60 includes at least three crystallization stages 61, 64 and 65. The operation of the crystallization stages is as follows:

[0098] Stage 1: Crystallizing carbonate-based co-solvent equivalents;

[0099] Stage 2: crystallizing a mixture of carbonate-based co-solvent equivalents, sodium phosphate and / or potassium phosphate;

[0100] Stage 3: Crystallization of the remaining sodium and / or potassium phosphate.

[0101] In this regard, the first crystallization stage 61 includes at least an evaporation stage, wherein water is evaporated from the solution 54 in an evaporation vessel. As the water evaporates from the solution 54, the carbonate-based co-solvent equivalent begins to form crystals of the carbonate-based co-solvent equivalent in the solution 54. At the same time, the concentration of sodium phosphate and / or potassium phosphate in the solution 54 increases.

[0102] Water is evaporated from the solution 54 until the sodium phosphate and / or potassium phosphate begins to form crystals. At this point, evaporation of water from the solution is terminated (heating is terminated). This maximizes the recovery of the carbonate-based co-solvent and minimizes the extent to which the sodium phosphate and / or potassium phosphate affects the purity of the recovered carbonate-based co-solvent. At least a portion of the water evaporated from the solution 54 can be reused 55 as wash water 52.

[0103] It should be appreciated that the type of evaporation vessel used will depend on the scale. For small-scale operations, a single-effect evaporator is suitable. In contrast, industrial-scale processes will typically employ multi-stage evaporation. The resulting vapor is collected and used as process water 55 or sent to a mechanical vapor recompression system to generate steam that can be used to initially heat the evaporator.

[0104] When the evaporation stage is operated to form crystals of carbonate-based flux equivalent in solution 54, the first crystallization stage 61 will include a second separation (e.g., filtration) stage in which a substantially liquid-free solid 62 is separated from the remaining liquid. The solid 62 contains the carbonate-based flux and may also include contaminants introduced with the water 52 in the water wash stage 50.

[0105] Typically, the resulting solids 62 are recycled, constituting at least a portion of the molten carbonate-based flux 22 introduced into the mixing stage 20. This reduces the mass of fresh carbonate-based flux 22 required for the process 10. Advantageously, this can reduce the cost of the process 10.

[0106] The solution 66 separated from the solid 62 contains sodium and / or potassium phosphates, and some carbonate-based co-solvent equivalents. The solution 66 is sent to a second crystallization stage 64, where the remaining carbonate-based co-solvent equivalents and some sodium and / or potassium phosphates are crystallized from the solution 66.

[0107] In this regard, the second crystallization stage 64 includes at least an evaporation stage, wherein water is evaporated from the solution 66 in an evaporation vessel. As the water evaporates from the solution 66, the remaining carbonate-based co-solvent equivalents are crystallized from the solution 66. At the same time, sodium phosphate and / or potassium phosphate form sodium phosphate and / or potassium phosphate crystals in the solution 66.

[0108] Typically, water is evaporated from solution 66 until all carbonate-based co-solvent equivalents are precipitated as crystals. At least a portion of the water evaporated from solution 66 may be reused 55 as wash water 52.

[0109] As noted above, it will be appreciated that the type of evaporation vessel employed will depend on the scale, with single effect evaporators being suitable for small scale, while industrial scale processes employ multi-stage evaporation.

[0110] When the evaporation stage is operated to form crystals of carbonate-based co-solvent equivalents and sodium and / or potassium phosphate in solution 66, the second crystallization stage 64 will include a second separation (e.g., filtration) stage, wherein a substantially liquid-free solid 67 is separated from the remaining liquid. The solid 67 comprises carbonate-based co-solvent equivalents and sodium and / or potassium phosphate. Typically, this solid 67 is discarded as waste.

[0111] It should be noted that, in the case where the flux contains chloride, part of the carbonate component in the flux will crystallize in stage 61, and the remaining carbonate component in the flux will crystallize in stage 64. However, the chloride equivalent will not crystallize in stage 61 or stage 64. In this regard, after the carbonate component of the carbonate flux has completed crystallization simultaneously with the phosphate, the remaining solution still contains the chloride component of the flux and sodium phosphate and / or potassium phosphate. The remaining solution 63 mainly contains sodium phosphate and / or potassium phosphate (and chloride when the flux contains chloride), which is sent to the third crystallization stage 65. The third crystallization stage 65 includes at least an evaporation stage, wherein water is evaporated from the solution 63 in an evaporation vessel. As water evaporates from the solution 63, the remaining sodium phosphate and / or potassium phosphate crystallize therefrom.

[0112] Typically, water is evaporated from solution 63 until all of the sodium phosphate and / or potassium phosphate has crystallized. At least a portion of the water evaporated from solution 63 can be reused 55 as wash water 52.

[0113] As noted above, it will be appreciated that the type of evaporation vessel employed will depend on the scale, with single effect evaporators being suitable for small scale, while industrial scale processes utilize multi-stage evaporation.

[0114] When the evaporation stage is operated to form sodium phosphate and / or potassium phosphate crystals, the third crystallization stage 65 may include a second separation (e.g., filtration) stage in which substantially liquid-free solids 57 are separated from residual liquid 69. The solids 57 comprise sodium phosphate and / or potassium phosphate. The residual liquid 69 may be collected for reuse in the process, e.g., as process water.

[0115] As mentioned above, when the carbonate-based flux contains chloride, the chloride component tends not to crystallize in stage 65. In this regard, the liquid 69 still contains the chloride component of the carbonate-based flux, which is evaporated again to regenerate NaCl (and / or KCl, as the case may be).

[0116] The crystallized sodium phosphate and / or potassium phosphate 57 is collected and can be sold directly as a byproduct of method 10. Alternatively, the crystallized sodium phosphate and / or potassium phosphate 57 can be subjected to further processing to separate the sodium phosphate and potassium phosphate (when both are present). The recovered sodium phosphate and potassium phosphate can be sold as separate byproducts. For example, sodium phosphate can be used as a fertilizer or fertilizer raw material, and can also be used as a cleaning agent, lubricant, food additive, detergent and degreasing agent.

[0117] Therefore, it should be recognized that depending on the flux composition, the multi-stage crystallization and separation stages are different. In particular, the number of stages can vary with the ratio of the flux and the flux to the mineral. The operating conditions of each crystallization stage will also vary depending on the composition of the carbonate-based flux and the concentration of the phosphate (sodium and / or potassium). For example, with respect to separation, the concentration is very important relative to the concentration of the solvent. In this regard, the concentration will change continuously with evaporation relative to the concentration of the solvent composition in the solution 54. For more complex carbonate-based fluxes (i.e., fluxes containing more components), more crystallization stages may be required. In addition, each stage also needs to be carefully controlled to maximize the recovery rate of each component of the carbonate-based flux and sodium phosphate and / or potassium phosphate. In this regard, the flux and phosphate recovery stage 60 may be quite complex because the carbonate-based flux may include several components, resulting in different relative concentrations of the components of the carbonate-based flux and sodium phosphate and / or potassium phosphate.

[0118] For example, when the carbonate-based flux comprises sodium carbonate and sodium chloride, the carbonate-based flux equivalent crystallized in the first crystallization stage may comprise only sodium carbonate due to the relative concentrations of sodium carbonate and sodium chloride and the higher solubility of sodium chloride. As described above, in the second crystallization stage, a mixed sodium carbonate / sodium phosphate product is produced, and in the third crystallization stage, sodium phosphate is crystallized. The solution separated from the sodium phosphate crystals still comprises sodium chloride, while the solvent and phosphate recovery stage 60 comprises one or more additional crystallization stages in which sodium chloride is recovered.

[0119] Likewise, it should be appreciated that the amount of each crystallized product (carbonate-based flux 62, waste 67, sodium phosphate and / or potassium phosphate 57) will vary, depending on the composition of the carbonate-based flux and the concentration of phosphate (sodium and / or potassium) in solution 54 relative to the flux composition.

[0120] The crushed solids 56, now depleted of carbonate-based flux, produced in the water wash stage, e.g., by filtration, contain primarily new (possibly carbonate and / or oxide) rare earth element compounds and phosphate rock residues. The flux-lean solids 56 are collected and sent to and subjected to an acid wash stage 70. The acid wash stage 70 is operated to substantially dissolve the rare earth element compounds from the flux-lean solids 56.

[0121] In the acid wash stage 70, the lean co-solvent solid 56 is washed with an acid 72. The washing is carried out in batches or continuously in one or more vessels at ambient temperature and pressure. The washing is carried out using nitric acid at a concentration of about 1M. The inventors speculate that other strong acids may also be used to wash the lean co-solvent solid 56, such as hydrochloric acid or sulfuric acid. The concentration of the acid is selected to provide a high recovery rate of the rare earth element compound into the solution.

[0122] Since the generated rare earth element compounds are soluble in acid, the rare earth element compounds are dissolved from the solid 56 by washing the co-solvent-lean solid 56 with acid 72 , thereby generating a rare earth element-containing solution 72 and a solid (ie, rare earth-lean) residue 74 .

[0123] The solution 72 containing the rare earth elements is separated 75 from the solid residue 74, for example by filtering or decanting. Without wishing to be bound by theory, the inventors speculate that the solid residue 74 should primarily contain cerium (IV) oxide (CeO2), thorium oxide (ThO2) and some phosphates. The solid residue 74 is collected. If the solid residue 74 contains thorium, it is radioactive and must be properly handled. For example, the solid residue 74 can be discarded as radioactive waste. Alternatively, if it is economical to do so, the solid residue 74 can be subjected to further processing to recover thorium and / or cerium therefrom. The recovered thorium and / or cerium can be sold as a product. The remaining residue (i.e., the solid remaining after the thorium and / or cerium are extracted) is discarded as waste.

[0124] The solution 72 containing rare earth elements can be further processed 80 using methods known in the art (e.g., adding oxalic acid) to produce a rare earth element product 82. This further processing can be performed as part of the method disclosed herein. In addition, the solution containing rare earth elements can be pumped or transported to another facility for further processing, but this option is more expensive. Another alternative option is to send the solution 72 containing rare earth elements to an evaporation stage, wherein a solid substantially free of liquid containing rare earth elements is formed. Then, the solid substantially free of liquid containing rare earth elements is transported to a separate facility, wherein individual rare earth elements are separated. Compared with liquids, the logistics of transporting solids are more convenient, and the unit cost of rare earth elements is significantly lower.

[0125] As mentioned above, phosphate ores containing rare earth elements often contain varying amounts of uranium and thorium. These elements are radioactive and therefore require proper handling and disposal.

[0126] The uranium dissolves during the pickling stage 70 and thus enters the rare earth element containing solution 72. This is described in further detail in Examples 3-7 below.

[0127] Without wishing to be bound by theory, the inventors hypothesize that, in order to safely recover uranium, uranium can be precipitated as an oxide from a solution 72 containing rare earth elements. The solution 72 is then filtered and the uranium oxide solids are collected for safe disposal. Uranium can also be removed from the solution 72 using established techniques. The uranium-free solution can be further processed to recover the rare earth elements therein.

[0128] Depending on the conditions of the heat treatment stage 30, the thorium is either primarily present in the residue 74 or primarily in the rare earth element-containing solution 72. This is described in further detail in Examples 3-7 below.

[0129] When thorium is left in the residue 74, no further treatment is required. The residue 74 is then radioactive and requires appropriate treatment. When thorium is present in the solution 72 containing rare earth elements, thorium can be removed from the solution, for example by precipitating the thorium as thorium oxide. The thorium oxide solid is then filtered and collected for safe disposal. Without wishing to be bound by theory, the inventors speculate that an alternative to precipitation and filtration may be to use electrolysis to separate thorium from the solution. However, the inventors point out that electrolysis is costly due to electricity costs and may not be economical on a large scale. The thorium-free solution can be further processed to recover the rare earth elements therein.

[0130] It should be appreciated that method 10 is not limited to phosphate ores containing rare earth elements. The method can be applied to other ores similarly formed from or soluble in carbonate melts. For example, the method can be used to recover elements such as niobium, tantalum, titanium or zircon from oxide ores such as pyrochlore, columbite, tantalite, niobium ore, ilmenite and zircon. The method can also be used to recover rare earth elements from silicate heterogeneous stones, and to recover lithium from spodumene. It should be appreciated that this list is not exhaustive, as there are many minerals that carbonate melts can dissolve.

[0131] For oxide and silicate ores, method 10 includes the same stages as described above. However, in the heat treatment stage 30, without wishing to be bound by theory, the inventors speculate that the oxide / silicate ore will dissolve in the molten carbonate-based flux, thereby forming simple oxides therein. For example, pyrochlore [Ca2Nb2O7] can form oxides Nb2O5 and CaO (or CaCO3). The simple oxides can then be separated from the residue, for example, by density separation. When oxide and / or silicate ores are used as feeds to method 10, the carbonate-based flux will typically contain one or more chlorides. In addition, it is believed that adding silica and / or phosphates to the carbonate-based flux can increase the solubility of the oxide / silicate ore. This can increase the recovery rate of metals recovered from these minerals. In some cases, the temperature of the heating step can be as high as about 800°C or more. Such a temperature may be required to promote the reaction between the ore and the flux. For example, in the case of recovering zirconium from zircon, the heating step may require a temperature of up to about 850°C. Example

[0132] Some non-limiting examples will now be described to further illustrate the method of recovering rare earth elements from phosphate ore using a carbonate-based flux. In Examples 3-8, a powdered phosphate ore is mixed with an appropriate carbonate-based flux in a platinum crucible. The sample is placed in a box furnace at 50°C above the expected melting temperature of the carbonate-based flux and left for a predetermined time to allow the ore to completely dissolve. After removing the sample from the furnace, it is crushed into a fine powder using a mortar and pestle until it is uniform in size.

[0133] About 0.105 g of each sample was then added to 10 mL of warm tap water in a 15 mL centrifuge tube and placed in an ultrasonic bath for 2 min. The resulting solution was then left to stand for 2 h. After 2 h, the aqueous solution was collected for analysis. The remaining residue in the test tube was weighed and added to 10 mL of warm 1M HNO3 and then placed in an ultrasonic bath for 2 min. The acid solution was then left to stand for 2 h. After 2 h, the acid solution was collected for analysis.

[0134] Two sets of solutions collected from the leaching process were analyzed using an Agilent ICP-OES 5110. To ensure that the concentrations met the instrument's analytical parameters, each leachate fraction was diluted 1:10 with dilute HNO3. Five rare earth element standards were prepared using standard solution ICP-OESIQ1 at concentrations of 0.1ppm, 1ppm, 10ppm, 50ppm, and 100ppm.

[0135] The recovery of phosphate minerals was calculated using the concentrations of rare earth elements in water and nitric acid solutions.

[0136] For each rare earth element, the recovery was calculated as the ratio of the mass extracted to the mass originally in the ore. The recovery calculations assumed that 100% of the rare earth elements were originally deposited by the phosphate in the ore and therefore could be extracted by the process.

[0137] The method was tested using three different phosphate minerals: synthetic monazite, naturally occurring monazite, and naturally occurring xenotime. The synthetic monazite was prepared in the laboratory from analytical grade reagents. Example 1 illustrates the research method.

[0138] In addition, three different carbonate-based fluxes were tested: a eutectic Na2CO3-K2CO3-KCl composition, a composition based on naturally occurring carbonate melts from the Lengai volcanic eruption, and a eutectic Na2CO3-NaCl composition. All fluxes were prepared in the laboratory from analytical grade reagents. Example 2 illustrates the research method.

[0139] A first set of experiments was run in which different ratios of phosphate minerals to carbonate-based fluxes were tested, including the use of no carbonate-based flux. These experiments were run using two flux compositions: a eutectic Na2CO3-K2CO3-KCl composition and a composition based solely on Lengai volcanic carbonate melts. For consistency, the mixture of phosphate minerals and carbonate-based fluxes was placed in a box furnace at a temperature 50°C above the melting point of the corresponding flux for 3 h.

[0140] A second set of experiments was performed on synthetic monazite only, where the predetermined time of placing the samples in the box furnace at 50°C above the melting temperature of the carbonate-based flux was varied. These experiments were performed using only the eutectic Na2CO3-K2CO3-KCl composition as flux and at a 5:1 flux to phosphate mineral mass ratio.

[0141] Figure 2 The composition of the rare earth elements in ppm for the synthetic monazite, natural monazite, and xenotime samples used in the experiments is provided. Natural xenotime contains the full set of rare earth elements, but is enriched in heavy rare earth elements. Natural monazite contains the full set of rare earth elements, but is enriched in light rare earth elements. Synthetic monazite is synthesized to contain only light rare earth elements plus Yb.

[0142] A third set of experiments was conducted on natural monazite only, using a eutectic Na2CO3-NaCl carbonate-based flux with a flux to phosphate mineral mass ratio of 4:1. The samples were placed in a box furnace at 650°C, and the predetermined time for placing the samples in the box furnace was varied.

[0143] The applicability of the method to other (non-phosphate) ores was tested and demonstrated by Example 8. In particular, the method was tested using zircon (ZrSiO4) and a eutectic Na2CO3-NaCl carbonate-based flux.

[0144] Example 1 - Preparation of synthetic monazite

[0145] A synthetic monazite mixture was produced for use in rare earth element extraction processes. This mixture is based on Rapp and Watson (1986) (Monazite solubility and dissolution kinetics: implications for the thorium and light rare earth chemistry of felsic magmas. Contributions to Mineralogy and Petrology, 94, 304–316. https: / / doi.org / 10.1007 / BF00371439 ) , but excluding CaO, ThO2 and U3O8. Table 1 below provides the composition of the synthetic monazite mixture. The mixture was produced using analytical grade reagents.

[0146] The reagent mixture is pressed into pellets and then fired overnight in an atmospheric pressure Gero gas mixing tube furnace at 1400°C in air. The pellets are removed, crushed, pressed into pellets again, and fired again. The purpose of the second firing is to redistribute the unreacted starting materials to increase the yield of monazite. Once the second firing is complete, the pellets are reduced to powder.

[0147] Table 1. Composition of synthetic monazite

[0148]

[0149]

[0150] Figure 3 This is a backscattered electron image of a synthetic monazite sample taken using a JEOL 8530F Plus electron probe microanalyzer. The image shows the presence of at least two different phases in the sample: a monazite phase 100 and a cerium oxide (CeO2) phase 102.

[0151] From the composition analysis, the Ce2O3 concentration of the monazite phase itself is almost 1 / 4 of the Ce2O3 concentration put into the monazite mixture before firing (microprobe shows about 7wt% in monazite and 26.6wt% in the monazite mixture). This means that only a part of the Ce is stored in the monazite. The rest of the Ce is stored in the form of oxides.

[0152] It should be recognized that since the Ce recovery calculations were initially based on the mass of Ce in the synthetic monazite mixture, the yield percentage values ​​for all (synthetic monazite) experiments were significantly lower than expected. This is because the majority of Ce present in synthetic monazite is CeO2 dissolved in the carbonate co-solvent.

[0153] Two different synthetic monazites were prepared. The first synthetic monazite was used in a first series of experiments that involved testing different carbonate-based fluxes and different ratios of flux to monazite. The second synthetic monazite was used in a second series of experiments that involved different heating times. Both synthetic monazites exhibited the same CeO2 phase.

[0154] The presence of the CeO2 phase is a direct consequence of the fact that the monazite is synthetic (prepared in a laboratory setting). This phase is not characteristic of naturally occurring monazite. Despite the presence of CeO2 impurities, rare earth elements were still observed to be extracted from the samples, indicating that the methods disclosed herein are effective.

[0155] Example 2 - Preparation of carbonate-based flux

[0156] All carbonate-based fluxes were prepared in the laboratory using analytical grade reagents. The first flux was based on Yan et al. (2019) (Preparation and Experimental Study of Three Element Mixed Molten Salt. IOP Conferences Series Materials Science Engineering. 585. https: / / doi.org / 10.1088 / 1757-899X / 585 / 1 / 012010 ) reported in the eutectic Na2CO3-K2CO3-KCl composition (referred to herein as "eutectic Na2CO3-K2CO3-KCl"). The second co-solvent is based on a simplified composition of carbonate melts from the eruption of Lengai volcano (referred to herein as "synthetic Lengai volcano"). The third co-solvent is based on the eutectic Na2CO3-NaCl composition.

[0157] To determine the melting point of the carbonate-based fluxes, a sample of each flux was pelletized and loaded onto a metal plate. The metal plate was then placed in a Linkam TS1400 heating stage connected to an Olympus BX60 microscope. The temperature of the heating stage was calibrated using a selected standard of H2O / CO2 fluid at -56.6°C, a series of organic compounds with a temperature span of 80-230°C, and silver at 962°C. All measurements were performed in a nitrogen atmosphere at a constant flow rate. A heating rate of 50°C / min was used from room temperature until about 50°C below the expected melting point. The heating rate was then slowed to 20°C / min for the next 40°C and then set to 6°C / min until the pellet began to change shape and "flow". This was defined as the melting point. The heating process was observed optically. The accuracy and precision of the instrument were monitored by comparing the melting points determined for the physical mixture of K2CO3 and Na2CO3 with those in the literature (Reisman, A., 1959. Heterogeneous equilibria in the system K2CO3–Na2CO3. Journal of the American Chemical Society 81, 807–811.). Table 2 shows the three carbonate co-solvent compositions and melting points.

[0158] Table 2. Compositions and melting points of three carbonate-based fluxes used for recovery of rare earth elements from phosphate ore.

[0159]

[0160] The melting point of synthetic Lengai flux is higher than that of carbonate melts from natural Lengai eruptions. This is because natural carbonate melts contain other elements, such as fluorides, which are not included in the synthetic analogues of Lengai flux for simplicity and safety reasons.

[0161] Example 3 - Synthetic Monazite:Carbonate Ratios

[0162] In the first set of experiments, synthetic monazite samples were mixed with eutectic Na2CO3-K2CO3-KCl and synthetic Lengai carbonate-based fluxes, respectively, and subjected to the experimental procedure described above. For the eutectic Na2CO3-K2CO3-KCl flux, the following flux-to-synthetic monazite mass ratios were tested: 0.2:1, 2.5:1, 3.3:1, 5:1, 10:1. For the synthetic Lengai flux, the following flux-to-synthetic monazite mass ratios were tested: 2.5:1, 3.3:1, 5:1. For comparison, the experimental procedure was also performed on samples with only synthetic monazite (i.e., without flux).

[0163] Figure 4 and Figure 5 The recoveries of La, Ce, Pr, Nd, Sm, Eu, Gd, and Y are shown when using eutectic Na2CO3-K2CO3-KCl and synthetic Lengai as carbonate-based co-solvents, respectively.

[0164] Figure 4 and Figure 5 All indicate that in order to extract rare earths from synthetic monazite, carbonate-based flux is necessary. In other words, in the absence of carbonate-based flux, the extracted rare earth elements are less than 1%. On the contrary, the effectiveness of the method of recovering rare earths using carbonate-based flux is demonstrated. The results show that under certain conditions, close to 100% of rare earths are extracted.

[0165] For the eutectic Na2CO3-K2CO3-KCl carbonate-based flux, the extraction rate increases with increasing ratio of carbonate-based flux to monazite. At a mass ratio of 10:1, essentially all of La, Pr, Nd, Eu, Gd and Y were extracted. Most of the Sm was also extracted. It is speculated that the (slightly) low recovery of Sm is an analytical artifact. The lowest extraction rates were observed for ratios 0.2:1 and 2.5:1, where about 50% of all elements except Ce were extracted. This suggests that a ratio of at least 2.5:1 is appropriate in order to extract at least 50% of the rare earth elements.

[0166] Commercially, the ratio of cosolvent to monazite is not too high because it means that a large amount of cosolvent is required. This can increase the cost of the cosolvent recovery stage 60 ( Figure 1 ), for example, a larger evaporator requires more energy. Therefore, it is noted that a balance between the need for co-solvent and the recovery of rare earth elements is required. It is also noted that if the recovery of rare earth elements is less than 100%, a portion of the solid residue 74 can be recycled back to the mixing stage 20 for further processing.

[0167] In all ratios of cosolvent to synthetic monazite, the extraction yield of Ce is significantly lower than that of other rare earth elements. Without wishing to be bound by theory, the inventors hypothesize that the low yield of Ce is due to the formation of an insoluble cerium oxide phase during the synthesis of synthetic monazite. As described in Example 1, the backscattered electron image ( Figure 3 ) indicates the presence of cerium oxide phase 102. Since the cerium oxide phase is insoluble in carbonate melts, Ce cannot be extracted using this method.

[0168] Under certain conditions (eg, a co-solvent to monazite ratio of 10:1), the Ce recovery was consistent with at least some Ce being extracted from the monazite.

[0169] When using synthetic Lengai carbonate-based fluxes ( Figure 5), when the flux to mineral ratio was 2.5:1 or greater, almost 100% recovery of all rare earth elements except Ce was observed. This indicates that Lengai carbonate-based fluxes can be effectively used to recover rare earth elements.

[0170] Likewise, the lower recovery of Ce compared to other REEs is due to the presence of cerium oxide, which accounts for the majority of Ce in the sample.

[0171] Comparison of the recoveries achieved with the eutectic Na2CO3-K2CO3-KCl and synthetic Lengai carbonate-based fluxes shows that the simpler eutectic Na2CO3-K2CO3-KCl mixture is able to recover essentially all of the rare earth elements from the phosphate rock. The advantage of the eutectic Na2CO3-K2CO3-KCl mixture is that the melting point of the flux is significantly lower than that of the synthetic Lengai, allowing heating to be performed at lower temperatures. The synthesis and recovery of the eutectic Na2CO3-K2CO3-KCl mixture is also simpler because it does not require the use of additional components such as SrCO3 or BaCO3. However, the rare earth recoveries using synthetic Lengai show that the method can be used with a wide range of carbonate-based flux compositions.

[0172] Example 4 - Monazite: Time Test

[0173] A time trial experiment was conducted on a mixture of synthetic monazite and a low eutectic Na2CO3-K2CO3-KCl carbonate-based solvent. The rare earth element recovery rates at different times are shown in Figure 2. Figure 7 shown.

[0174] For all rare earth elements, the recovery of each rare earth element as a function of heating time follows the same trend. In particular, the highest recovery occurs after 1 hour of heating. The lowest recovery occurs after 10 hours of heating. Interestingly, the recovery after 30 minutes of heating is only slightly higher than that after 10 hours of heating (<5%).

[0175] Without wishing to be bound by theory, the inventors speculate that in a very short time frame (e.g. < 1 h), the carbonate co-solvent does not have enough time to completely melt and completely dissolve the phosphate rock. Therefore, the rare earth elements are not released from the phosphate mineral into the carbonate mineral and are therefore unable to dissolve during the pickling process.

[0176] In contrast, at longer heating times, the inventors speculate that the low recovery is due to partial decarburization of the carbonate melt. It is well known that Na2CO3 begins to decarburize at around 500°C. Since the furnace temperature is about 625°C, some decarburization of the co-solvent can be expected. Decarburization causes Na2CO3 to decompose, thereby releasing CO2. This results in less carbonate available to dissolve monazite.

[0177] Example 5 - Natural Monazite: Solvent Ratio

[0178] In the next set of experiments, natural monazite samples were mixed with eutectic Na2CO3-K2CO3-KCl and subjected to the above experimental procedures. For each flux, the following flux to natural monazite mass ratios were tested: 10:1, 5:1, 3.3:1, 2.5:1. The scheduled time was 1 hour.

[0179] Figure 8 The recoveries of La, Ce, Pr, Nd, Sm, Gd, Y, Th, and U are shown for each mass ratio tested. The recoveries are almost the same for the mass ratios of cosolvent to natural monazite of 2.5:1 and 3.3:1. The composition of rare earth elements in natural monazite was previously determined ( Figure 2 ).

[0180] Carbonate-based fluxes are capable of extracting rare earth elements from natural monazite, and under certain conditions, recoveries of most elements approaching 100% can be achieved. The extraction yield of rare earth elements decreases with increasing carbonate-based flux to monazite ratio, with the exception of U. For U, the maximum yield occurs at a flux to monazite ratio of 3.3:1, and the yield decreases as the flux to monazite ratio decreases to 2.5:1.

[0181] For all elements, the highest extraction yields were observed at ratios of 2.5:1 and 3.3:1. At these mass ratios, essentially all of the La, Pr, Nd, Sm, Gd, and Y were extracted. The Gd yield percentage slightly less than 100% is believed to be an analytical artifact.

[0182] The amount of Th extracted from natural monazite was low, less than 20% for all carbonate cosolvent to monazite ratios tested. This suggests that most of the Th is present in the solid residue 74 (see Figure 1 ), because Th remains in the residue after pickling. It is speculated that this is because Th is 4+ The presence of ThO2 in its oxidized state results in the production of ThO2 during the cooling phase of the heat treatment 30. As is known, ThO2 is only slightly soluble in acid. Advantageously, this means that Th can be safely disposed of by disposing of the solid residue 74 as radioactive waste.

[0183] The Ce extraction rate of natural monazite is higher than that of synthetic monazite because a large amount of Ce in synthetic monazite is in the form of CeO2. This shows that this method is capable of recovering Ce from phosphate minerals. However, the extraction rate of Ce is low compared to other rare earth elements in all ratios of cosolvent to natural monazite. Ce can be recovered as Ce 4+ and Ce 3+ Two forms exist. Although Ce 3+Can form acid-soluble oxides, but Ce 4+ Forming acid-insoluble CeO2. Although Ce is usually mainly present in natural monazite as Ce 3+ However, it is speculated that the low Ce yield is due to Ce3 + Oxidized to Ce 4+ This occurs because both heating and melting occur in air.

[0184] However, incomplete extraction of Ce is not considered a major problem because Ce is relatively cheap and abundant compared to other rare earth elements. In addition, in some cases, a low extraction rate of Ce may be beneficial. This is because monazite contains high concentrations of Ce (>100,000 ppm on a normal basis). If Ce remains in the solid residue, the volume of rare earth element concentrate produced from solution 72 can be reduced, which can reduce associated transportation costs.

[0185] It should be noted that, if economical, the remaining solid residue 74 may be further processed to recover Th and / or Ce therefrom.

[0186] Example 6 - Natural Monazite: Flux Type

[0187] In this experiment, the effectiveness of a eutectic Na2CO3-NaCl carbonate-based co-solvent for the recovery of rare earth elements from natural monazite was tested. The experimental method described above was used. In the first experiment, the sample was kept at 650°C for a predetermined time of 1 hour. In the second experiment, the predetermined time was 2 hours. The yields of La, Ce, and Nd in each experiment are provided in the table below.

[0188] Table 3 Recovery of rare earth elements in natural monazite at different predetermined heating times

[0189]

[0190] When the heating time is 2 hours, the eutectic Na2CO3-NaCl carbonate-based co-solvent is able to extract more than 90% of La, about 90% of Nd and about 75% of Ce present in natural monazite. The lower recovery of Ce is also believed to be due to the formation of acid-insoluble CeO2 during the heat treatment stage.

[0191] Only the yields of La, Ce, and Nd were measured, since these elements are the main components of natural monazite samples (see Figure 2). It is important to note that other REEs found in monazite, including Pr, Sm, Eu, Gd, and Lu (albeit at lower concentrations), tend to be found in similar yields to La and Nd. Therefore, the eutectic Na2CO3-NaCl carbonate-based cosolvent is expected to be able to extract REEs other than La, Ce, and Nd from monazite as well.

[0192] These experiments demonstrate that the eutectic Na2CO3-NaCl carbonate-based flux is suitable for the recovery of rare earth elements from phosphate minerals such as monazite. It is important to note that this is beneficial because the cost of sodium-based reagents is much lower than that of potassium-based reagents. By using a flux containing only sodium-based reagents, the overall cost of the process can be reduced. However, the rare earth recovery using the eutectic Na2CO3-NaCl flux shows that a wider range of carbonate-based flux compositions can be used with this method.

[0193] Example 7 - Xenotime:Carbonate Ratio

[0194] In this set of experiments, natural xenotime samples were mixed with eutectic Na2CO3-K2CO3-KCl and synthetic Lengai carbonate-based fluxes, respectively, and subjected to the experimental procedure described above. For both fluxes, the following flux to synthetic monazite mass ratios were tested: 0.2:1, 2.5:1, 3.3:1, 5:1, 10:1, 20:1. The scheduled time was one hour. Based on previous analyses, the rare earth element composition ( Figure 2 ). For comparison, the experimental procedure was also carried out on a sample containing only xenotime (ie without flux). When no flux was used, the predetermined time was 3 hours.

[0195] Fig. 9 and Fig.10 The recoveries of rare earth elements from xenotime when mixed with eutectic Na2CO3-K2CO3-KCl and synthetic Lengai fluxes are shown at different ratios of flux to xenotime. When no flux was used, the recoveries of rare earth elements from xenotime were <1%, indicating that mixing xenotime with flux is necessary for the recovery of rare earth elements. The recoveries of rare earth elements are nearly identical for all mass ratios of flux to xenotime of 2.5:1 or greater, resulting in the overlap of several data sets in each figure.

[0196] When xenotime is mixed with the eutectic Na2CO3-K2CO3-KCl flux ( Fig. 9 ), when the mass ratio of the solvent to xenotime is greater than 0.2:1, the recovery rate of almost all rare earth elements is close to 100%.

[0197] The recoveries of U and Th were also measured because these elements are radioactive. For all co-solvent to xenotime ratios above 0.2:1, substantially all of the U was extracted from the xenotime. This means that U is present in the solution containing the rare earth elements. In a commercial-scale process, U needs to be removed from the solution (e.g., by precipitation) before the rare earth elements are recovered.

[0198] For some ratios of co-solvent to xenotime, the recovery of Th is less than 100%. Specifically, at ratios of 5:1, 3.3:1, and 2.5:1, the recovery of Th is about 40% to about 60%. This means that, depending on the heat treatment stage 30 ( Figure 1 ) operating conditions, Th is either in the solution 72 containing the rare earth elements or in the solid residue 74. If Th is in the solid residue 74, the residue can be disposed of as radioactive waste. On the other hand, if Th is in the solution 72, it can be removed from the solution (e.g., by precipitation or electrolysis) before recovering the rare earth elements.

[0199] Example 8 - Recovery of zirconium from natural zircon

[0200] In this experiment, a natural zircon sample was mixed with a low eutectic Na2CO3-NaCl flux. The ratio of the mass of the flux to the mass of the mineral was 5:1. 1.8 g of the mixed material was weighed. The mixture was kept at 850°C for 18 hours in a box furnace. After 18 hours, the mixture was quenched by turning off the power supply to the furnace. It should be noted that, compared with the conditions for monazite and xenotime, when the mineral is zircon, some experimental conditions, such as the predetermined temperature and time, must be improved. However, the inventors point out that the temperature of 850°C and the predetermined time of 18 hours are not optimized.

[0201] It was observed that during the heating process, the mass of the mixture lost about 67% by weight. Without wishing to be bound by theory, it is believed that this is due to decarburization during the heating process while the zircon reacts with the sodium carbonate and sodium chloride according to the following reaction formula:

[0202] ZrSiO4+2Na2CO3+NaCl→Na2ZrO3+Na2SiO3+2CO2+NaCl

[0203] To determine the minerals present after heat treatment, a small portion of the quenched product was loaded into epoxy resin and imaged using a scanning electron microscope (SEM). Care was taken to avoid sample hydration during preparation. The composition of the phases present was determined by energy dispersive spectroscopy (EDS). Representative SEM images are shown in Figure 2. Fig.11EDS analysis shows the presence of NaCl phase 202 and Na2ZrO3 phase 204. This supports the idea that zircon can be transformed into new Zr and Si compounds by heating in a co-solvent.

[0204] The remaining quenched product was leached with 200 mL of water in triplicate to ensure complete dissolution of the residual Na2CO3 and NaCl. It was observed that Na2CO3, Na2SiO3 and NaCl were all dissolved from the quenched product during the water wash.

[0205] Without wishing to be bound by theory, the inventors speculate that during the washing of the quench residue, the Na2ZrO3 phase is converted to ZrO(OH)2 according to the following reaction:

[0206] Na2ZrO3+H2O→ZrO(OH)2+Na2O

[0207] The Na2O then forms sodium hydroxide (NaOH) during the water wash and is therefore also dissolved from the quenched product.

[0208] To convert ZrO(OH)2 into ZrO2, the samples were calcined at 800℃ for 4 hours. The calcined solid samples were loaded into epoxy resin and examined by SEM and EDS. Representative SEM images are shown in Fig.12 EDS analysis showed that the calcined sample 206 consisted almost entirely (about 90% by weight) of ZrO2.

[0209] Although the acid leaching step was not performed in this experiment, the acid leaching step of the process is well understood by those skilled in the art. Since ZrO2 is known to be soluble in certain acids, such as nitric acid, hydrochloric acid, and sulfuric acid, it is expected that acid leaching will extract a significant proportion of Zr. Without wishing to be bound by theory, the inventors note that other components present, such as Hf, may also be extracted during the acid leaching of the calcined solid. Zr can then be separated from these other components (such as Hf) in the resulting solution using standard methods.

[0210] The experiment shows that the method is suitable for recovering certain metals from silicate and / or oxide ores containing certain metals. For example, the method is suitable for recovering zirconium from zircon.

[0211] The inventors also point out that reacting zircon with Na compounds to produce Na2ZrO3 (which is then converted to ZrO(OH)2 by washing) is a step in other metallurgical processing routes for zircon [I am cautious about the term "traditional" because commercial methods, i.e., traditional methods, are not always described in the literature, and I have not conducted a comprehensive review of the field]. However, these routes generally employ sintering, which may require higher operating temperatures. In contrast, this experiment shows that the method disclosed herein is capable of recovering zircon from zircon at lower temperatures, and it should be noted that the reaction conditions used in this example are not optimized.

[0212] Without departing from the spirit or scope of the present disclosure, changes and modifications may be made to the foregoing description. For example, these changes and modifications may be required when processing phosphate, oxide or silicate ores with different gangue minerals, or when applying different methods for removing uranium / thorium. In the following claims and the foregoing description of the method, unless the context requires otherwise by express or necessary implication, the word "comprise" or variations such as "comprises" or "comprising" are used in an inclusive sense, that is, to indicate the presence of the features described, but not to exclude the presence or addition of other features in various embodiments of the method.

Claims

1. A method for recovering one or more rare earth elements from a phosphate ore containing the one or more rare earth elements, the method comprising: a) mixing the phosphate rock containing one or more rare earth elements with a carbonate-based flux; b) subjecting the mixture to conditions such that the one or more rare earth elements are released from the phosphate rock and form one or more rare earth element compounds.

2. The method of claim 1 , wherein the conditions of b) comprise subjecting the mixture to a temperature that causes the carbonate-based flux to melt for a predetermined time, whereby the phosphate ore comprising one or more rare earth elements is substantially dissolved in the molten carbonate-based flux.

3. The method of claim 2, wherein the conditions of b) further comprise solidifying the resulting molten mixture after the predetermined time has elapsed, thereby forming the one or more rare earth element compounds as a solid.

4. The method of claim 2 or 3, wherein the elevated temperature is in the range of about 500°C to about 650°C.

5. The method of any one of claims 2-4, wherein the predetermined time is about 2 hours.

6. The process as claimed in any one of the preceding claims, wherein b) is carried out at ambient pressure.

7. A method as claimed in claim 3 or any one of claims 4 to 6 when dependent on claim 3, wherein the one or more rare earth element compounds obtained are separated from a solid residue.

8. The method of claim 7, wherein separating the rare earth element compounds from the solid residue comprises fragmenting the solid comprising one or more rare earth element compounds to produce fragmented solids.

9. The method of claim 8, wherein said separating said rare earth element compound from said solid residue further comprises washing said crushed solid with water to substantially dissolve residual carbonate-based flux therefrom.

10. A method as claimed in claim 9, wherein the wash water comprising dissolved residual carbonate-based flux is separated and further processed to recover said carbonate-based flux as a solid substantially free of liquid, for example by evaporation.

11. A method as claimed in claim 10, wherein solid carbonate-based flux substantially free of liquid is recycled to constitute at least a portion of the molten carbonate-based flux of a).

12. The method of any one of claims 9-11, wherein said separating said rare earth element compounds from said solid residue further comprises washing the resulting lean co-solvent solid with an acid to substantially dissolve said one or more rare earth element compounds therefrom, thereby producing a solution comprising said one or more rare earth elements and a residue.

13. The method of claim 12, wherein the acid has a concentration of about 1 M.

14. A method as claimed in claim 12 or 13, wherein the acid comprises a mineral acid such as nitric acid, hydrochloric acid or sulphuric acid.

15. The method of any one of claims 12-14, further comprising separating the solution comprising the one or more rare earth elements from the residue, such as by filtration, and optionally further processing the solution comprising the one or more rare earth elements to produce one or more rare earth element products.

16. A process as claimed in any one of the preceding claims, wherein the mixture of a) comprises a greater proportion by mass of the carbonate-based co-solvent than the phosphate ore comprising one or more rare earth elements.

17. The method of claim 16, wherein the ratio of the carbonate-based co-solvent to the phosphate rock by mass is at least 2:

1.

18. The method of any one of the preceding claims, wherein the phosphate rock comprises at least one of the minerals monazite, xenotime or apatite.

19. A method as claimed in any one of the preceding claims, wherein the carbonate-based flux comprises sodium carbonate and potassium carbonate.

20. The method of claim 19, wherein the carbonate-based co-solvent further comprises chloride in the form of at least one of sodium chloride or potassium chloride.

21. The method of claim 20, wherein the carbonate-based co-solvent comprises, by weight, about 30% sodium carbonate, about 50% potassium carbonate, and about 20% potassium chloride.

22. The method of any one of claims 1-18, wherein the carbonate-based co-solvent comprises sodium carbonate and sodium chloride.

23. The method of claim 22, wherein the carbonate-based co-solvent comprises about 60% sodium carbonate and about 40% sodium chloride by weight.

24. The method of any one of claims 19-23, wherein the carbonate-based co-solvent further comprises small amounts of other elements added.

25. A method as claimed in any one of claims 19 to 24, when referred to in any one of claims 10 to 15, wherein the separated wash water containing dissolved residual carbonate-based co-solvent also contains sodium phosphate and / or potassium phosphate, and the method further comprises separating the sodium phosphate and / or potassium phosphate therefrom.

26. A method as claimed in any preceding claim, wherein the ore comprising the one or more rare earth elements is pre-treated, for example by flotation or gravity separation, and the pre-treated ore is mixed with the carbonate-based flux in a).

27. A method for recovering a metal or metals from an ore containing the metal or metals oxides, the method comprising: i) mixing an oxide ore comprising one or more metals with a carbonate-based flux; ii) subjecting the mixture to conditions such that the metal or metals are released from the oxide ore and form one or more carbonate or oxide compounds comprising the metal or metals.

28. A process as claimed in claim 27, wherein the resulting one or more metal carbonate or oxide compounds are separated from the remainder of the mixture.

29. The method of claim 27 or 28, wherein the oxide ore comprises at least one of the minerals pyrochlore, columbite, niobite, tantalite or ilmenite, and the metal or metals comprise at least one of the metals niobium, tantalum or titanium.

30. A method as claimed in any one of claims 27 to 29, further aspects of the method being as defined in any one of claims 2 to 25.

31. The method of any one of claims 27-30, wherein the carbonate-based co-solvent comprises one or more of chloride, silica, phosphate.

32. A method for recovering a metal or metals from a silicate ore containing the metal or metals, the method comprising: i) mixing the silicate ore containing a certain metal or certain metals with a carbonate-based flux; ii) subjecting the mixture to conditions such that the metal or metals are released from the silicate ore and form one or more carbonate or oxide compounds comprising the metal or metals.

33. The process of claim 31, wherein the one or more metal carbonate or oxide compounds obtained are separated from the residue of the mixture.

34. The method of claim 31 or 32, wherein the silicate ore comprises at least one of the minerals zircon, pyroxene and spodumene, and the metal or metals comprise at least one of zirconium, at least one rare earth element or lithium.