Preparation method of 2D / 2D mesoporous Co3O4 / BiOCl photo-thermal antibacterial agent

By compounding 2D BiOCl nanosheets with 2D mesoporous Co3O4, a 2D/2D mesoporous Co3O4/BiOCl p-n junction is constructed, which solves the problems of BiOCl carrier radiation recombination and narrow spectral response range, and significantly improves photothermal conversion efficiency and antibacterial properties. performance, achieving efficient photothermal antibacterial effect.

CN118844461APending Publication Date: 2024-10-29SHANGHAI ACAD OF AGRI SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410815454.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The carrier radiation recombination phenomenon of simple BiOCl nanosheets is serious, and the narrow spectral response range results in low photothermal conversion efficiency, which limits its application in the field of antibacterial.

Method used

Composite 2D BiOCl nanosheets and 2D mesoporous Co3O4 through electrostatic self-assembly to construct a 2D/2D mesoporous Co3O4/BiOCl p-n junction. The photoinduced self-heating effect and mesoporous structure of Co3O4 are used to increase the reaction temperature and active sites, and promote photogeneration. Carrier migration and transfer.

Benefits of technology

It significantly improves the charge separation efficiency and bacterial adsorption capacity of the material, enhances the photothermal antibacterial activity, and achieves efficient photothermal conversion and antibacterial effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118844461A_ABST
    Figure CN118844461A_ABST
Patent Text Reader

Abstract

The invention discloses a 2D / 2D mesoporous Co3O4 / BiOCl photo-thermal antibacterial agent and a preparation method, the Co3O4 / BiOCl photo-thermal antibacterial agent is composed of 2D mesoporous Co3O4 and 2D BiOCl nanosheets, and the 2D mesoporous Co3O4 and the 2D BiOCl nanosheets are combined in an electrostatic self-assembly mode to form a 2D / 2D p-n junction. The preparation method comprises the following steps: adding Co3O4 and BiOCl into isopropanol, and carrying out ultrasonic treatment to uniformly disperse the Co3O4 and BiOCl; and after stirring the obtained suspension for a period of time, centrifuging and drying to obtain the Co3O4 / BiOCl p-n junction photo-thermal antibacterial agent. The Co3O4 / BiOCl p-n junction photo-thermal antibacterial agent provided by the invention has very high carrier separation efficiency and bacterium adsorption capacity, and also has good photo-thermal conversion efficiency. The preparation method is simple and high in controllability, and large-scale production is easy to realize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention improves the charge separation efficiency and photothermal antibacterial performance of BiOCl by constructing a 2D / 2D p-n junction, and specifically relates to a method for combining 2D BiOCl nanosheets and 2D mesoporous Co 3 O 4 The invention belongs to the technical field of materials science and technology to construct a pn junction photothermal antibacterial agent by means of electrostatic self-assembly. Background Art

[0002] As people pay more and more attention to environmental hygiene, their awareness of sterilization and disinfection has also increased significantly. The widespread use of antibiotics by humans has led to increased bacterial resistance. The speed of research and development of antibacterial materials has been unable to cope with the increasing resistance and resistance of bacteria. Human society may face the danger of large-scale bacterial infections that cannot be cured. The design and development of new antibacterial materials is imminent.

[0003] Traditional sterilization treatment technologies, including physical disinfection, chemical disinfection and biological disinfection, cannot effectively kill all bacteria because of their high stability and low biodegradability. Therefore, it is very necessary to develop environmentally friendly and feasible antibacterial technologies. In recent years, photothermal catalysis has become a promising antibacterial strategy. It relies on photoresponsive materials with wide spectrum absorption to absorb sunlight, which can bring two effects: first, the photoresponsive material converts the absorbed sunlight into heat, thereby increasing the temperature of the reaction system, thereby destroying the membrane and protein of the bacteria, causing the bacteria to lose activity; on the other hand, the photoresponsive material can produce photoactive oxidative species under the irradiation of sunlight, which can kill bacteria at the same time. The core of realizing this technology lies in the development of photothermal materials with both high photothermal conversion efficiency and carrier separation efficiency.

[0004] Heterostructure construction is considered to be an effective strategy to improve the efficiency of carrier separation of materials. Among them, 2D / 2D heterojunctions have a large specific surface area and abundant active sites, which are conducive to promoting the antibacterial reaction. At the same time, the unique layered morphology of 2D materials increases their close interfacial contact with bacterial membranes. In addition, the layered structure of 2D semiconductors helps photogenerated carriers migrate from the interior to the surface reaction sites, which improves the efficiency of photocatalytic sterilization. BiOCl, as a typical 2D layered material, has been used in the antibacterial field. However, pure BiOCl has problems such as low carrier separation efficiency and narrow light response range, which limits its application in the antibacterial field. Therefore, it is necessary to find a material with a wide spectral response and an energy level matching that of BiOCl to composite it with it to construct a 2D / 2D heterojunction.

[0005] Co 3 O 4It is a p-type semiconductor material with a narrow bandgap and strong light absorption ability, especially the absorption in the near-infrared region, which can convert light into heat, increase the reaction temperature, and is conducive to antibacterial reaction. Inspired by this, we used an electrostatic self-assembly method to combine 2D BiOCl nanosheets and 2D mesoporous Co 3 O 4 Composite, prepared 2D / 2D mesoporous Co 3 O 4 / BiOCl photothermal antibacterial agent, this unique 2D / 2D stacking structure provides great advantages: on the one hand, Co 3 O 4 The photoinduced self-heating effect can increase the temperature of the reaction system and promote the antibacterial reaction; secondly, the mesoporous Co 3 O 4 The introduction of can increase the specific surface area of ​​the material, increase the active sites, and improve the material's ability to adsorb bacteria; at the same time, p-type Co 3 O 4 The pn junction can be formed with n-type BiOCl. The pn junction has a built-in electric field, which is beneficial to promote the migration of photogenerated carriers and improve the antibacterial performance. Based on the above advantages, we innovatively proposed a 2D BiOCl nanosheet and 2D mesoporous Co 3 O 4 Compounding to build 2D / 2DCo 3 O 4 / BiOCl pn junction, which is expected to show enhanced photothermal antibacterial activity. Summary of the invention

[0006] The technical problem to be solved by the present invention is that the carrier radiation recombination phenomenon of pure BiOCl nanosheets is serious, and the narrow spectral response range leads to low photothermal conversion efficiency, which is not conducive to its photothermal antibacterial efficiency.

[0007] In order to solve the above technical problems, the present invention discloses a 2D / 2D mesoporous Co 3 O 4 Preparation method of BiOCl photothermal antibacterial agent using 2D BiOCl nanosheets and 2D mesoporous Co 3 O 4 The composite is formed by electrostatic self-assembly. The unique 2D / 2D structure and pn junction construction of the material effectively promote the separation / transfer of charges. At the same time, the mesoporous structure improves the adsorption capacity of the composite material to bacteria, and the wide spectrum absorption can significantly increase the reaction temperature and promote the antibacterial reaction. The specific steps include:

[0008] Step 1): 2D mesoporous Co 3 O 4and 2D BiOCl nanosheets were added to isopropanol and ultrasonicated for half an hour to obtain a suspension;

[0009] Step 2): After the mixture is stirred for a period of time, it is centrifuged and the supernatant is discarded to obtain a precipitate;

[0010] Step 3): The obtained precipitate is placed in a drying oven and dried to obtain Co 3 O 4 / BiOCl photothermal antibacterial agent.

[0011] The 2D mesoporous Co 3 O 4 2D BiOCl nanosheets can be prepared using existing technology, and the preparation method is described in Small 2024, 2401601 and Sustainable Materials and Technologies, 2024, 39, e00825.

[0012] Preferably, in step 1), Co 3 O 4 The amount of added is 30-70 mg, the amount of added BiOCl is 30-70 mg, and the volume of isopropanol is 5-20 mL.

[0013] Preferably, the stirring time in step 2) is 4-12 hours.

[0014] Preferably, the drying temperature in step 3) is 60-120° C. and the drying time is 8-12 hours.

[0015] 2D / 2D mesoporous Co synthesized by the present invention 3 O 4 / BiOCl photothermal antibacterial agent not only has excellent charge separation efficiency and bacteria adsorption performance, but also has good photothermal conversion efficiency. This invention provides a new idea for designing highly active photothermal antibacterial agents and has great potential in the fields of animal husbandry and aquaculture. At the same time, this method is simple to operate, highly controllable, and easy to achieve large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The BiOCl and Co obtained in Example 1 3 O 4 , and Co 3 O 4 / X-ray diffraction (XRD) patterns of BiOCl samples;

[0017] Figure 2 The BiOCl and Co obtained in Example 1 3 O 4 , and Co3 O 4 Transmission electron microscopy (TEM) images and EDX spectra of the / BiOCl samples;

[0018] Figure 3 The BiOCl and Co obtained in Example 1 3 O 4 , and Co 3 O 4 Infrared thermal imaging photos of / BiOCl samples;

[0019] Figure 4 The BiOCl and Co obtained in Example 1 3 O 4 , and Co 3 O 4 Photocurrent and electrochemical impedance spectroscopy of / BiOCl samples;

[0020] Figure 5 The BiOCl and Co obtained in Example 1 3 O 4 , and Co 3 O 4 Photocatalytic antibacterial experiment of / BiOCl sample under xenon lamp. DETAILED DESCRIPTION

[0021] In order to make the present invention more clearly understood, preferred embodiments are described in detail below with reference to the accompanying drawings.

[0022] Example 1

[0023] A 2D / 2D mesoporous Co 3 O 4 / BiOCl photothermal antibacterial agent and preparation method thereof, specifically comprising the following steps:

[0024] (1) Preparation of 2D BiOCl nanosheets: First, 30 mL of distilled water was added to a beaker, followed by 2 mmol of bismuth nitrate pentahydrate and 2 mmol of potassium chloride. After being stirred for 1.5 hours, the mixture was poured into a 50 mL polytetrafluoroethylene-lined stainless steel autoclave and kept at 160°C for 24 hours. After the reaction solution was cooled to room temperature, the precipitate was obtained by centrifugation and washed three times with deionized water, and then dried at 60°C for 12 hours.

[0025] (2) Preparation of 2D mesoporous Co 3 O 4 :Configuration consists of 0.5g Co(NO 3 ) 2 6H 2O, 0.5 g MCM-48 and 5 mL ethanol were prepared, stirred continuously for 1 h, and then the ethanol was evaporated in an oven at 100 ° C, and the obtained solid was calcined at 550 ° C for 6 h. The burned sample powder was then washed with 2 M sodium hydroxide solution at 50 ° C with stirring, and the template was removed by centrifugation, which was repeated three times. The obtained product was washed with deionized water until neutral and dried at 80 ° C overnight.

[0026] (3) Preparation of Co 3 O 4 / BiOCl heterojunction: The prepared Co 3 O 4 (50 mg) and BiOCl (50 mg) were added to 10 mL of isopropanol, and the mixture was stirred for 12 h, then centrifuged, the supernatant was discarded to obtain a precipitate, and finally dried at 60 °C for 12 h to obtain the product.

[0027] The XRD diffraction patterns of the sample powders were measured by D / max 200PC X-ray diffractometer. 3 O 4 and Co 3 O 4 The XRD diffraction patterns of the / BiOCl composite materials are shown in Figure 1 As shown. It can be seen that pure BiOCl shows obvious diffraction peaks at 11.96°, 24.12°, 25.88°, 32.52°, 33.52°, 36.56°, 49.72°, 55.16°, 58.64°, etc., corresponding to the (001), (002), (101), (110) (102), (003), (113), (104), (212) planes of tetragonal BiOCl (JCPDS No.06-0249), respectively. In addition, pure Co 3 O 4 The diffraction peaks of Co are also consistent with the standard spectrum (PDF#34–1003). 3 O 4 The XRD spectrum of the / BiOCl composite material has similar diffraction peaks to that of pure BiOCl, but it is difficult to observe Co 3 O 4 The diffraction peaks may be due to Co 3 O 4 The diffraction intensity is low. However, this does not affect the 3 O 4 The conclusion that the nanosheets were successfully composited was established, and subsequent characterization also confirmed this.

[0028] The morphology of the samples was observed using a transmission electron microscope (FEI tecnaiG2F30, FEI Company, USA). Figure 2 As shown in a, BiOCl presents a rectangular nanosheet structure. Figure 2 b is Co 3 O 4 TEM image, it can be observed that Co 3 O 4 It also shows a nanosheet structure, with many holes distributed on the nanosheet, showing a mesoporous structure. 3 O 4 TEM images of the / BiOCl composites ( Figure 2 c) It can be seen that Co with 2D mesoporous structure 3 O 4 Nanosheets are stacked on 2D BiOCl nanosheets, indicating that 2D / 2D mesoporous Co 3 O 4 Successful construction of / BiOCl heterojunction. Figure 2 TEM image of d shows that BiOCl nanosheets and 2D mesoporous Co 3 O 4 The nanosheets have clear contact interfaces. High-resolution TEM (HRTEM) further revealed that the Co 3 O 4 The clear lattice fringes with spacing of 0.34 nm and 0.24 nm are attributed to the (101) plane of BiOCl and the Co 3 O 4 The (311) plane ( Figure 2 e). Figure 2 The EDX spectrum of f confirmed that Co 3 O 4 The presence of Co, Bi, Cl and O in 2D / 2D mesoporous Co 3 O 4 Successful construction of / BiOCl heterojunction.

[0029] To study Co 3 O 4 , BiOCl and Co 3 O 4 The photothermal conversion capability of / BiOCl composite materials is measured by using infrared thermal imaging to record the temperature changes of the materials under simulated sunlight. Figure 3 As shown, within 0-10min, Co 3 O 4 , BiOCl and Co 3 O 4 / BiOCl composite material temperature change record, it can be seen that Co3 O 4 The temperature of the / BiOCl composite material increases rapidly under illumination, and its temperature is also the highest within the same illumination time, indicating that its photothermal conversion efficiency is the highest.

[0030] To further understand Co 3 O 4 The photogenerated carrier transfer / separation efficiency of the / BiOCl composites was tested by transient photocurrent response and electrochemical impedance spectroscopy (EIS). Figure 4 a shows BiOCl, Co 3 O 4 and Co 3 O 4 The transient photocurrent response of / BiOCl. The results show that compared with pure BiOCl and Co 3 O 4 In comparison, Co 3 O 4 The / BiOCl composite material has a higher photocurrent intensity, proving that the electron transfer / separation efficiency in this composite material is significantly improved. The electrochemical impedance spectroscopy of the sample is shown in Figure 2. Figure 4 b. Generally speaking, the smaller the arc radius of the Nyquist curve, the higher the efficiency of photogenerated carrier transfer / separation. 3 O 4 The semicircle radius of the Nyquist plot of the / BiOCl composite is larger than that of the original BiOCl and Co 3 O 4 are all small, indicating that the charge transfer resistance of the composite material is smaller, which is beneficial to improving the charge transfer / separation efficiency.

[0031] Co 3 O 4 , BiOCl and Co 3 O 4 The / BiOCl composite material was used as a photothermal antibacterial agent to conduct antibacterial experiments on Gram-negative bacteria (Escherichia coli) under simulated sunlight. Figure 5 As shown in a, with the extension of illumination time, the number of bacteria gradually decreased, among which Co 3 O 4 When the / BiOCl composite material was used as an antibacterial agent, the number of bacteria decreased fastest. Figure 5 b shows Co 3 O 4 The antibacterial rate of the / BiOCl composite material reached 97.52% at 4 min, and the antibacterial effect was significantly better than that of Co 3 O 4 And BiOCl pure sample. Figure 5 c is the growth of the colonies on the LB culture dish during photothermal antibacterial treatment. Co3 O 4 The number of colonies treated with the / BiOCl composite material basically disappeared, and after 8 minutes of irradiation, the antibacterial rate was close to 100%, showing excellent photothermal antibacterial ability.

[0032] Example 2

[0033] The difference between this embodiment and embodiment 1 is that: 3 O 4 The added amounts of BiOCl and BiOCl were 30 mg and 70 mg respectively, and the rest of the contents were exactly the same as described in Example 1.

[0034] The photothermal catalytic antibacterial performance test shows that the Co 3 O 4 The antibacterial rate of the / BiOCl photothermal antibacterial agent under the same conditions is 94.7%, which is lower than the antibacterial performance of the material obtained in Example 1.

[0035] Example 3

[0036] The difference between this embodiment and embodiment 1 is that: 3 O 4 The added amounts of MgSO4 and BiOCl were 70 mg and 30 mg respectively, and the rest of the contents were exactly the same as described in Example 1.

[0037] The photothermal catalytic antibacterial performance test shows that the Co 3 O 4 The antibacterial rate of the / BiOCl photothermal antibacterial agent under the same conditions is 90.6%, which is lower than the antibacterial performance of the material obtained in Example 1.

[0038] In summary, the present invention provides a 2D / 2D mesoporous Co 3 O 4 / BiOCl photothermal antibacterial agent, which has excellent charge separation efficiency and bacteria adsorption capacity, and also has good photothermal conversion efficiency, can rapidly heat up under the irradiation of simulated sunlight, and exhibits excellent photothermal antibacterial performance. The preparation method is simple, highly controllable, and easy to achieve large-scale production.

Claims

1. A method for preparing a 2D / 2D mesoporous Co3O4 / BiOCl photothermal antibacterial agent, characterized in that: The 2D mesoporous Co3O4 and 2DBiOCl nanosheets are compounded by an electrostatic self-assembly method to construct a Co3O4 / BiOCl pn junction. The specific steps include: Step 1): Add 2D mesoporous Co3O4 and 2D BiOCl nanosheet materials into isopropanol and ultrasonicate for half an hour to obtain a suspension; Step 2): After the mixture is stirred for a period of time, it is centrifuged and the supernatant is discarded to obtain a precipitate; Step 3): The obtained precipitate is placed in a drying oven and dried to obtain a Co3O4 / BiOCl photothermal antibacterial agent.

2. The method for preparing the 2D / 2D mesoporous Co3O4 / BiOCl photothermal antibacterial agent according to claim 1, characterized in that: In the step 1), the amount of Co3O4 added is 30-70 mg, the amount of BiOCl added is 30-70 mg, and the volume of isopropanol is 5-20 mL.

3. The method for preparing the 2D / 2D mesoporous Co3O4 / BiOCl photothermal antibacterial agent according to claim 1, characterized in that: The stirring time in step 2) is 4-12 hours.

4. The method for preparing the 2D / 2D mesoporous Co3O4 / BiOCl photothermal antibacterial agent according to claim 1, characterized in that: The drying temperature in step 3) is 60-120° C. and the drying time is 8-12 hours.