Sodium ferric phosphate pyrophosphate / carbon composite positive electrode material, preparation thereof, pole piece and battery
Through the airgel structure and paste electrode preparation method of sodium iron pyrophosphate/carbon composite material, the problems of poor conductivity and insufficient thermal stability of the sodium-ion battery cathode material are solved, and the high energy density and cycle of the sodium-ion battery are achieved. Stability, it has the application potential of replacing and supplementing lithium-ion batteries.
Patent Information
- Application Number
- CN202410909322.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-29
AI Technical Summary
Existing cathode materials for sodium-ion batteries have problems such as poor conductivity, insufficient thermal stability, and immature large-scale production, which limits their application in replacing and supplementing lithium-ion batteries.
Sodium iron pyrophosphate/carbon composite material (Na4Fe3(PO4)2(P2O7)@C) is prepared through starch hydrogel to form an aerogel structure, combined with heat treatment and the use of conductive polymers to improve the conductivity and conductivity of the material. Thermal stability, and the electrode active material loading capacity is increased through the paste electrode preparation method.
It has achieved low resistance and excellent electrochemical properties of sodium-ion battery cathode materials, improved energy density and cycle stability, and has industrial application prospects.
Smart Images

Figure CN118851130A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a sodium iron phosphate pyrophosphate / carbon composite positive electrode material and a preparation method thereof, a pole piece and a battery. Background Art
[0002] At present, lithium metal resources are facing the problem of uneven reserves and distribution. As a major producer and consumer of lithium-ion batteries, my country is highly dependent on the import of lithium resources. Therefore, actively exploring other new secondary batteries that can replace and supplement lithium-ion batteries has important strategic significance and practical application value. The reserves of metallic sodium on the earth are very abundant. Its element reserves in the earth's crust rank fourth. Sodium and lithium are in the same main group in the periodic table and show similar physical and chemical properties. In addition, the working principle of sodium-ion batteries is very similar to that of lithium-ion batteries. It mainly relies on the embedding and de-embedding of sodium ions in positive and negative electrode materials to realize the transfer of charge energy. Therefore, sodium-ion batteries have become a beneficial supplement to lithium-ion batteries due to their abundant resource reserves and low cost of raw materials.
[0003] As early as the 1980s, research on lithium-ion batteries and sodium-ion batteries began. Among them, lithium-ion batteries were first widely used in portable electronic devices. With the continuous improvement of their technology, they gradually dominated scientific research and commerce; while sodium-ion batteries were limited by the slow kinetic characteristics of sodium ions and the lack of suitable negative electrode materials, and their development was relatively slow. In recent years, with the continuous expansion of electrochemical energy storage demand and the continuous rise in lithium raw material prices, the research boom of sodium-ion batteries is gradually emerging.
[0004] At present, the more mainstream sodium-ion battery cathode materials are mainly divided into three types: transition metal oxides, Prussian blue and polyanions. Among them, the energy density of transition metal oxide sodium-ion battery cathode materials is relatively high, but the cost of raw materials is still relatively high; Prussian blue cathode materials need to be prepared by wet method at low temperature / normal temperature, and the product crystal structure is prone to defects and easy to carry crystal water, which is not conducive to the cycle performance of the electrode, and its large-scale production technology is still immature and imperfect; and polyanion compounds have become the most promising type of sodium-ion battery cathode material due to their excellent structural stability, high safety and suitable voltage platform. Among them, due to the low cost of iron resources and the relatively simple preparation method, iron-based polyanion sodium-ion cathode materials are one of the most popular polyanion sodium-ion battery cathode materials.
[0005] Among them, layered oxides and Prussian blue materials have poor thermal stability and pose safety hazards when the battery is at high temperature. The sodium iron phosphate pyrophosphate material has good thermal stability and therefore exhibits higher safety performance. However, the sodium iron phosphate pyrophosphate material has the problem of poor intrinsic conductivity of polyanion compounds, and it is necessary to control the material preparation to improve its conductivity. The aerogel NFPP material is prepared by surface carbon coating and nano-sizing, which can improve its conductivity and achieve improved electrochemical performance. The high-temperature sintering structure of the sodium iron phosphate pyrophosphate material is difficult to control. Its synthesis temperature is 550°C, and it is impossible to achieve complete carbonization of the surface-coated carbon layer to form an oxygen-rich carbon oxide layer, but the surface-coated carbon layer can effectively inhibit particle growth. The surface area of the nano-scale surface carbon-coated polyanion positive electrode material is high, and the solid content is limited when the electrode slurry is prepared, resulting in a limited active material loading of the prepared electrode sheet, which cannot increase the energy density. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the defects of the positive electrode materials in the above-mentioned prior art, and provide a sodium iron pyrophosphate / carbon composite positive electrode material and its preparation, pole piece and battery. The Na4Fe3(PO4)2(P2O7)@C (abbreviated as NFPP@C) aerogel positive electrode material provided by the present invention has a rich network pore structure, so that the active material can be fully infiltrated and contacted with the electrolyte, which is conducive to the diffusion of sodium ions in the positive electrode, showing lower resistance and better electrochemical performance.
[0007] The present invention provides a method for preparing a sodium iron phosphate pyrophosphate / carbon composite positive electrode material, which comprises the following steps:
[0008] (1) adding starch to a mixed solution of sodium salt, iron salt and phosphate, stirring, gelatinizing and aging to obtain a starch hydrogel;
[0009] (2) The starch hydrogel is dried to obtain a NFPP@C aerogel precursor, which is then heat treated to obtain a sodium iron pyrophosphate / carbon composite positive electrode material.
[0010] In step (1), the type of the sodium salt can be selected from one or more of sodium carbonate, sodium oxalate and sodium nitrate.
[0011] In step (1), the type of the iron salt can be selected from ferric nitrate and / or ferric oxalate.
[0012] In step (1), the type of the phosphate can be selected from one or more of ammonium phosphate, ammonium hydrogen phosphate and diammonium phosphate.
[0013] In step (1), preferably, the sodium salt, the iron salt and the phosphate are weighed in a stoichiometric ratio to maintain a Na:Fe:P molar ratio of 4:3:4. More preferably, a stoichiometric ratio of 5% excess sodium source material is adopted.
[0014] In step (1), the solvent in the mixed solution may be deionized water. + , Fe 3+ PO4 3- .
[0015] In step (1), the amount of starch used may be 4-10%, preferably 4-5%, such as 4.67%, 4.75%, 4.77% or 4.80%, where % refers to the mass percentage of starch in the mixed solution.
[0016] In step (1), the gelatinization can be carried out in a water bath. Stirring is maintained during the gelatinization process. 3- It can promote starch to form a hydrosol state.
[0017] In step (1), the gelatinization temperature may be 80-100°C, for example 95°C.
[0018] In step (1), the gelatinization time may be 10-60 min, for example 30 min.
[0019] In step (1), the aging can be carried out in an ice bath.
[0020] In step (1), the aging time may be 2-4 hours, for example 3 hours.
[0021] In step (2), the drying may be freeze-drying.
[0022] Wherein, in the freeze-drying, the freezing temperature may be -15--25°C, for example -18°C.
[0023] Wherein, in the freeze-drying, the freezing time may be 2-8 hours, for example 3 hours.
[0024] Wherein, in the freeze-drying, the drying time may be 12-48 hours, for example 24 hours.
[0025] In step (2), the heat treatment may be carried out in a two-stage heating method of carbonization and calcination.
[0026] The carbonization temperature may be 250-350°C, for example 300°C.
[0027] The heating rate to the carbonization temperature may be 2-5°C / min, for example 3°C / min.
[0028] The carbonization time may be 2-8 hours, for example 6 hours.
[0029] The calcination temperature may be 500-600°C, for example 550°C.
[0030] The heating rate to the calcination temperature may be 2-5°C / min, for example 3°C / min.
[0031] The calcination time may be 4-10 hours, for example 10 hours.
[0032] In step (2), the heat treatment may be performed under a reducing atmosphere.
[0033] The reducing atmosphere may be a hydrogen-argon mixed atmosphere, such as a 5% H2 / Ar mixed atmosphere.
[0034] In step (2), the sodium iron phosphate pyrophosphate / carbon composite positive electrode material is preferably in the form of an aerogel.
[0035] The present invention also provides a sodium iron phosphate pyrophosphate / carbon composite positive electrode material, which is prepared by the above preparation method.
[0036] In the present invention, the sodium iron phosphate pyrophosphate / carbon composite positive electrode material is preferably in the form of an aerogel.
[0037] In the present invention, the particle size of the sodium iron pyrophosphate / carbon composite positive electrode material is preferably 1-7 μm.
[0038] The present invention also provides a method for preparing a positive electrode sheet, which comprises the following steps:
[0039] (1) mixing the above-mentioned positive electrode material, polymer and conductive agent, adding NMP to prepare an electrode paste slurry; the solid content of the electrode paste slurry is 70-85%;
[0040] (2) The electrode paste slurry is pressed into a film, and the film is then placed on an aluminum foil for a second pressing to obtain a positive electrode sheet.
[0041] In step (1), the mass ratio of the positive electrode material to the polymer is preferably 80:(15-20), for example 80:17.
[0042] In step (1), the mass ratio of the positive electrode material to the conductive agent is preferably 80:(1-5), for example 80:3.
[0043] In step (1), the polymer may be one or more of polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl alcohol, polypropylene alcohol and styrene-butadiene rubber, for example, "polyvinyl alcohol and polytetrafluoroethylene" or "polypropylene alcohol and polytetrafluoroethylene".
[0044] In a preferred embodiment, polyvinyl alcohol and polytetrafluoroethylene are used as polymers, and the mass ratio of polytetrafluoroethylene to polyvinyl alcohol is 10:7.
[0045] In a preferred embodiment, polypropylene alcohol and polytetrafluoroethylene are used as polymers, and the mass ratio of polypropylene alcohol to polytetrafluoroethylene is 10:7.
[0046] In a preferred embodiment, polypropylene alcohol and polytetrafluoroethylene are used as polymers, and the mass ratio of polypropylene alcohol to polytetrafluoroethylene is 8:9.
[0047] In step (1), the conductive agent may be one or more of conductive carbon black, carbon nanotubes and graphene, such as conductive carbon black.
[0048] In step (1), the solid content of the electrode paste slurry may be 75-85%, for example 80%.
[0049] In step (2), the equipment used for both pressing steps can be a hot press.
[0050] The temperature of the hot press can be controlled at 70-90°C, such as 75°C or 85°C.
[0051] The pressure of the hot press can be controlled within the range of 1-10 kN. The setting parameters of the two pressings can be independently selected within the above range. During the pressing process, the pressure can be gradually increased and pressed multiple times to obtain an electrode sheet with uniform thickness. For example, three pressings are performed in sequence at pressures of 1 kN, 5 kN, and 8 kN.
[0052] In step (2), the pressing may further include a drying operation.
[0053] The drying temperature may be 90-120°C, for example 105°C.
[0054] The drying time may be 6-24 hours, for example 12 hours.
[0055] In step (2), the positive electrode plate is an electrode plate with aluminum foil as the base.
[0056] In step (2), the thickness of the positive electrode plate may be 60-120 μm.
[0057] The present invention also provides a positive electrode plate, which is prepared by the above preparation method.
[0058] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0059] The reagents and raw materials used in the present invention are commercially available.
[0060] The positive and progressive effects of the present invention are:
[0061] 1. The Na4Fe3(PO4)2(P2O7)@C(NFPP@C) aerogel cathode material provided by the present invention has a rich network pore structure, so that the active material can fully infiltrate and contact with the electrolyte, which is conducive to the diffusion of sodium ions in the cathode, showing lower resistance and better electrochemical performance. The raw materials of this method are cheap and easy to obtain, easy to implement, and have industrial application prospects.
[0062] 2. Furthermore, the present invention also provides a method for preparing a paste electrode, which is to prepare an electrode film by hot pressing, and then further hot pressing and attaching it to an aluminum foil to form an electrode. Commonly used electrode binders do not have conductive properties. This method uses a conductive polymer to replace a part of the traditional binder, while increasing the solid content of the electrode slurry, which can effectively increase the loading amount of the electrode active material and improve the energy density. BRIEF DESCRIPTION OF THE DRAWINGS
[0063] Figure 1 Schematic diagram of the preparation method for paste electrodes.
[0064] Figure 2 This is the SEM image of the NFPP@C aerogel positive electrode material prepared in Example 9.
[0065] Figure 3 This is the SEM image (magnification) of the NFPP@C aerogel positive electrode material prepared in Example 9.
[0066] Figure 4 The cycling performance of the battery using the NFPP@C aerogel cathode material prepared in Example 9 at a rate of 0.1C.
[0067] Figure 5 This is the rate performance of the battery of the NFPP@C aerogel positive electrode material prepared in Example 9.
[0068] Figure 6 This is the charge and discharge curve of the battery using the NFPP@C aerogel cathode material prepared in Example 9 at a rate of 0.1C. DETAILED DESCRIPTION
[0069] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0070] Example 1
[0071] 1. Preparation of aerogel sodium iron pyrophosphate cathode material
[0072] 1.1. Dissolve 8.50 g of sodium nitrate, 30.30 g of ferric nitrate nonahydrate and 12.00 g of ammonium dihydrogen phosphate in 250 mL of deionized water to obtain a mixed aqueous solution.
[0073] 1.2. Weigh 15g of industrial starch and add it to the above solution. Stir to obtain starch emulsion.
[0074] 1.3. Place the starch emulsion in a 95℃ water bath for gelatinization for 30 minutes. Keep stirring during the gelatinization process to finally form a hydrosol state.
[0075] 1.4. After the gelatinization process is completed, the starch hydrosol is poured into a container and placed in an ice bath for 3 hours to obtain a starch hydrogel after aging.
[0076] 1.5. The obtained starch hydrogel was frozen at -18°C for 3 hours and then freeze-dried for 24 hours to obtain a starch-based NFPP@C aerogel precursor.
[0077] 1.6. The aerogel precursor was placed in a vacuum tube furnace with a 5% H2 / Ar mixed atmosphere, heated to 300°C at a heating rate of 3°C / min, kept at 300°C for 6 hours, and then heated to 550°C at a rate of 3°C / min, kept at 550°C for 10 hours, and finally obtained Na4Fe3(PO4)2(P2O7)@C(NFPP@C) aerogel product. The product was transferred to a dryer for storage.
[0078] 2. Preparation of conductive polymer positive electrode film (positive electrode sheet)
[0079] 2.1. Prepare electrode paste slurry according to the mass ratio of NFPP@C aerogel positive electrode material: polyvinyl alcohol: polytetrafluoroethylene: conductive carbon black at 80:10:7:3, add appropriate amount of NMP to adjust the solid content of the electrode paste to 80%, transfer the mixed paste to a sealed bag, and use a hot press to initially press it into a uniform film; then take out the film and place it on aluminum foil, and further hot press to obtain an electrode film with aluminum foil as the base. The hot pressing temperature is controlled at 75°C, and the pressure is 1kN, 5kN, and 8kN respectively. Press three times to obtain an electrode sheet with uniform thickness. See the schematic diagram for details. Figure 1 .
[0080] 2.2. Transfer the electrode sheet to a vacuum drying oven and dry it at 105°C for 12 hours. Cut it into electrode discs with a diameter of 10 mm, weigh it, and transfer it to a glove box to be used as working electrode sheets.
[0081] Example 2 (Replacing the Sodium Source Material)
[0082] In step 1.1, the solute is 5.30 g of sodium carbonate, 30.30 g of ferric nitrate nonahydrate and 12.00 g of ammonium dihydrogen phosphate, and the remaining steps are the same as in Example 1.
[0083] Example 3 (Replacing the Sodium Source Material)
[0084] In step 1.1, the solute is 6.70 g sodium oxalate, 30.30 g ferric nitrate nonahydrate and 12.00 g ammonium dihydrogen phosphate (Na:Fe:P molar ratio is 4:3:4), and the remaining steps are the same as in Example 2.
[0085] Example 4 (Adjusting the Sodium Source Ratio)
[0086] In step 1.1, the solute is 7.03 g sodium oxalate, 30.30 g ferric nitrate nonahydrate and 12.00 g ammonium dihydrogen phosphate (Na:Fe:P molar ratio is 4.2:3:4, and the sodium source material is in excess of 5%), and the remaining steps are the same as in Example 3.
[0087] Example 5 (increasing the proportion of carbon source)
[0088] In step 1.2, the mass of industrial starch weighed is 18 g, and the remaining steps are the same as those in Example 4.
[0089] Example 6 (Increasing the freezing time)
[0090] In step 1.5, the precursor is frozen at -18°C for 6 hours, and the remaining steps are the same as in Example 5.
[0091] Example 7 (Replacing the electrode paste polymer)
[0092] The mass ratio of the electrode paste slurry in step 2.1 is NFPP@C aerogel positive electrode material: polypropylene alcohol: polytetrafluoroethylene: conductive carbon black = 80:10:7:3, and the remaining steps are the same as in Example 6.
[0093] Example 8 (Adjusting the ratio of electrode paste slurry)
[0094] The mass ratio of the electrode paste slurry in step 2.1 is NFPP@C aerogel positive electrode material: polypropylene alcohol: polytetrafluoroethylene: conductive carbon black = 80:8:9:3, and the remaining steps are the same as in Example 7.
[0095] Example 9 (Adjusting the hot pressing temperature)
[0096] The hot pressing temperature in step 2.1 is 85°C, and the remaining steps are the same as in Example 8.
[0097] Example 10 (Aerogel NFPP@C material with starch as carbon source, conventional coating method to prepare pole piece)
[0098] Step 2 is changed to a conventional electrode sheet preparation method to obtain a positive electrode sheet. Prepare an electrode slurry with a mass ratio of positive electrode material: conductive carbon black: binder of 85:8:7, and apply it on aluminum foil by blade coating. Place the aluminum foil in an oven and dry it at 80°C for 2 hours, then transfer it to a vacuum drying oven and dry it at 105°C for 12 hours. After rolling, cut it into electrode discs with a diameter of 10 mm, weigh it, and transfer it to a glove box for use as a working electrode sheet. The remaining steps are the same as in Example 1.
[0099] Comparative Example 1 (Preparation of NFPP material without adding carbon source by conventional solid phase method and preparation of pole piece by conventional coating method)
[0100] 1. Preparation of positive electrode material by solid phase method: 8.50g sodium nitrate, 30.30g ferric nitrate nine hydrate, 12.00 After being thoroughly mixed with a ball mill, g of ammonium dihydrogen phosphate was transferred to a corundum crucible and heated at 300°C for 6 hours in an inert atmosphere of 5% H2 / Ar mixed atmosphere, and then heated to 550°C for 10 hours to finally obtain Na4Fe3(PO4)2(P2O7) product.
[0101] 2. Use conventional electrode sheet preparation methods to coat the positive electrode sheet. Prepare the electrode slurry according to the mass ratio of positive electrode material: conductive carbon black: binder of 85:8:7, and apply it on the aluminum foil by blade coating. Place the aluminum foil in an oven and dry it at 80°C for 2 hours, then transfer it to a vacuum drying oven and dry it at 105°C for 12 hours. After rolling, cut it into electrode discs with a diameter of 10 mm, weigh it, and transfer it to the glove box for use as working electrode sheets.
[0102] Comparative Example 2 (Using glucose as the carbon source aerogel NFPP@C material, conventional coating method to prepare the pole piece)
[0103] In step 1, 15 g of glucose was used as the carbon source material.
[0104] Step 2 is changed to a conventional electrode sheet preparation method to obtain a positive electrode sheet, and an electrode slurry is prepared according to a mass ratio of positive electrode material: conductive carbon black: binder of 85:8:7, and coated on aluminum foil by blade coating. The aluminum foil is placed in an oven and dried at 80°C for 2 hours, then transferred to a vacuum drying oven and dried at 105°C for 12 hours, rolled, cut into electrode discs with a diameter of 10 mm, weighed, and transferred to a glove box for standby use as a working electrode sheet; the remaining steps are the same as in Example 1.
[0105] Comparative Example 3 (Aerogel NFPP@C material using citric acid as a carbon source)
[0106] In step 1, 15 g of citric acid is used as the carbon source material, and the remaining steps are the same as in Example 1.
[0107] Effect Example 1 Microstructure
[0108] Figure 2 and Figure 3 This is a SEM image of the NFPP@C aerogel cathode material prepared in Example 9. From the figure, it can be seen that the prepared material is a spherical particle with a particle size of about 1 to 7 μm, and the porous carbon network structure shuttles around the particles, which improves the electronic conductivity. In addition, the surface carbon coating layer can also effectively prevent the agglomeration and adhesion of the NFPP material and inhibit the growth of NFPP particles.
[0109] Effect Example 2 Electrochemical Performance
[0110] Assembly and testing of button cells:
[0111] Assemble a button half-cell based on sodium sheet to test and evaluate the electrochemical performance of the prepared material: select conventional 1M NaPF6 electrolyte, assemble CR 2016 button cell in the order of positive electrode sheet, separator, and negative electrode sheet, the above electrode sheet is the positive electrode, the metal sodium sheet is the negative electrode, and Whatman glass fiber is the separator. Connect the battery to the battery test system and perform charge and discharge tests in the range of 1.5V to 4V.
[0112] Table 1
[0113]
[0114] It can be seen from Examples 1-10 that when the positive electrode material prepared in the present invention is used in a battery, its 0.1C reversible capacity can reach 75.6-101.1 mAh / g, its 0.5C reversible capacity can reach 61.3-89.1 mAh / g, and its capacity retention rate after 200 cycles is 78.0-94.7%. Among them, the cycle performance, rate performance and charge-discharge curve of the battery of the NFPP@C aerogel positive electrode material prepared in Example 9 are as follows: Figure 4-Figure 6 shown.
[0115] According to the comparison between Example 1 and Example 10, when other conditions remain unchanged, the preparation method using the paste electrode is more effective than the preparation method using the conventional coating.
[0116] According to Comparative Example 1 and Comparative Example 3, when both methods for preparing paste electrodes are used, the present invention uses starch as a carbon source, and the reversible capacity and capacity retention rate of the obtained product are significantly better than those of the product using citric acid as a carbon source.
[0117] According to the comparison of Example 10 and Comparative Example 2, under the same preparation method of the positive electrode plate, the reversible capacity and capacity retention rate of the product prepared by the present invention using starch as the carbon source are significantly better than those of the product using glucose as the carbon source.
Claims
1. A method for preparing a sodium iron pyrophosphate / carbon composite positive electrode material, characterized in that: It includes the following steps: (1) adding starch to a mixed solution of sodium salt, iron salt and phosphate, stirring, gelatinizing and aging to obtain a starch hydrogel; (2) The starch hydrogel is dried to obtain a NFPP@C aerogel precursor, which is then heat treated to obtain a sodium iron pyrophosphate / carbon composite positive electrode material.
2. The method for preparing the sodium iron phosphate pyrophosphate / carbon composite positive electrode material according to claim 1, characterized in that: One or more of the following conditions are met: a. In step (1), the type of the sodium salt is selected from one or more of sodium carbonate, sodium oxalate and sodium nitrate; b. In step (1), the type of the iron salt is selected from ferric nitrate and / or ferric oxalate; c. In step (1), the type of the phosphate is selected from one or more of ammonium phosphate, ammonium hydrogen phosphate and diammonium phosphate; d. In step (1), the sodium salt, the iron salt and the phosphate are weighed in a stoichiometric ratio to maintain a Na:Fe:P molar ratio of 4:3:4; preferably, a stoichiometric ratio of 5% excess sodium source material is adopted; e. In step (1), the amount of starch used is 4-10%, preferably 4-5%, for example 4.67%, 4.75%, 4.77% or 4.80%, where % refers to the mass percentage of starch in the mixed solution.
3. The method for preparing the sodium iron phosphate pyrophosphate / carbon composite positive electrode material according to claim 1, characterized in that: One or more of the following conditions are met: a. In step (1), the gelatinization is carried out in a water bath; b. In step (1), the gelatinization temperature is 80-100°C; c. In step (1), the gelatinization time is 10-60 min; d. In step (1), the aging is carried out in an ice bath; e. In step (1), the aging time is 2-4 h; f. In step (2), the drying is freeze-drying; g. In step (2), the heat treatment adopts a two-stage heating method of carbonization and calcination; h. In step (2), the heat treatment is carried out under a reducing atmosphere.
4. The method for preparing the sodium iron phosphate pyrophosphate / carbon composite positive electrode material according to claim 3, characterized in that: One or more of the following conditions are met: a. In the freeze-drying process, the freezing temperature is -15--25°C; b. During the freeze drying, the freezing time is 2-8h; c. In the freeze-drying process, the drying time is 12-48 hours; d. The carbonization temperature is 250-350°C; e. The heating rate of heating to the carbonization temperature is 2-5°C / min; f. The carbonization time is 2-8h; g. The calcination temperature is 500-600°C; h. The heating rate of the heating to the calcination temperature is 2-5°C / min; i. The calcination time is 4-10h.
5. A sodium iron phosphate pyrophosphate / carbon composite positive electrode material, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 4; Among them, the sodium iron phosphate pyrophosphate / carbon composite positive electrode material is preferably in an aerogel state; the particle size of the sodium iron phosphate pyrophosphate / carbon composite positive electrode material is preferably 1-7 μm.
6. A method for preparing a positive electrode sheet, characterized in that: It includes the following steps: (1) Mixing the positive electrode material as claimed in claim 5, a polymer and a conductive agent, and adding NMP to prepare an electrode paste slurry; the solid content of the electrode paste slurry is 70-85%; (2) The electrode paste slurry is pressed into a film, and the film is then placed on an aluminum foil for a second pressing to obtain a positive electrode sheet.
7. The method for preparing a positive electrode sheet according to claim 6, characterized in that: One or more of the following conditions are met: a. In step (1), the mass ratio of the positive electrode material to the polymer is preferably 80:(15-20), for example 80:17; b. In step (1), the mass ratio of the positive electrode material to the conductive agent is preferably 80:(1-5), for example 80:3; c. In step (1), the polymer is one or more of polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl alcohol, polypropylene alcohol and styrene-butadiene rubber, for example, "polyvinyl alcohol and polytetrafluoroethylene" or "polypropylene alcohol and polytetrafluoroethylene"; d. In step (1), the conductive agent is one or more of conductive carbon black, carbon nanotubes and graphene, such as conductive carbon black; e. In step (1), the solid content of the electrode paste slurry is 75-85%.
8. The method for preparing a positive electrode sheet according to claim 6, characterized in that: Polyvinyl alcohol and polytetrafluoroethylene are used as polymers, and the mass ratio of polytetrafluoroethylene to polyvinyl alcohol is 10:7; Alternatively, polypropylene alcohol and polytetrafluoroethylene are used as polymers, and the mass ratio of polypropylene alcohol to polytetrafluoroethylene is 10:7; Alternatively, polypropylene alcohol and polytetrafluoroethylene are used as polymers, and the mass ratio of the polypropylene alcohol to the polytetrafluoroethylene is 8:
9.
9. The method for preparing a positive electrode sheet according to claim 6, characterized in that: One or more of the following conditions are met: a. In step (2), both pressing operations are performed using a hot press; Preferably, the temperature of the heat press is controlled at 70-90°C; Preferably, the pressure of the hot press is controlled at 1-10 kN; more preferably, the pressure is gradually increased during the pressing process and pressed multiple times to obtain an electrode sheet with uniform thickness; for example, pressing is performed three times in sequence at pressures of 1 kN, 5 kN, and 8 kN; b. In step (2), the thickness of the positive electrode plate is 60-120 μm.
10. A positive electrode sheet, characterized in that: It is prepared by the preparation method described in any one of claims 6 to 9.
Citation Information
Patent Citations
Mixed crystal type polyanionic phosphate positive electrode material for sodium ion battery and preparation method of mixed crystal type polyanionic phosphate positive electrode material
CN113675390A
Positive pole piece and preparation method thereof, energy storage device and power utilization device
CN116741944A
Secondary carbon coated ferric sodium pyrophosphate composite material and preparation method thereof
CN116845215A
Sodium ferric phosphate pyrophosphate positive electrode material, preparation method thereof, positive electrode plate and sodium battery
CN116914117A
Sodium ferric phosphate pyrophosphate positive electrode material, preparation method thereof and sodium ion battery
CN117239118A
Cited By
Preparation method and application of surface carbon-coated sodium iron phosphate pyrophosphate positive electrode material
CN119786585A
NFPP-based positive electrode material, preparation method thereof and sodium ion battery
CN121748339A