Density and granularity control method for hollow glass beads
By calculating and determining the foaming dose and spheroidization temperature, the density and particle size of hollow glass microspheres can be prepared with controllability, which solves the problem of poor performance of domestic microspheres and improves the performance of deep-sea buoyancy materials.
Patent Information
- Application Number
- CN202411037403.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-29
AI Technical Summary
The density and particle size control of domestic hollow glass beads are poor, resulting in poor performance of domestic buoyancy materials and their inability to meet the high-intensity needs of deep-sea exploration.
Through theoretical derivation and actual production experience, combined with the glass powder method preparation process, the foaming dose and spheroidization temperature node are determined to achieve controllable preparation of the density and particle size of hollow glass beads. The density of the glass powder, the volume and outer diameter of the beads are used. Calculate other parameters to ensure the linear effect of the foaming agent.
The highly controllable preparation of hollow glass microspheres is achieved, which is suitable for the needs of deep-sea solid buoyancy materials at different depths and improves the performance level of domestic buoyancy materials.
Smart Images

Figure CN118851546A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hollow glass microsphere preparation, and particularly relates to a density / particle size control technology for preparing high-performance hollow glass microspheres for solid buoyancy materials by a glass powder method. Background Art
[0002] Solid buoyancy materials are one of the key technologies for human deep-sea exploration, and are mainly prepared by adding resin and lightening agent. Hollow glass microspheres have the characteristics of low density and high strength, and are the preferred additive for solid buoyancy materials. The filling volume fraction can reach more than 70%, and it is the core raw material for preparing high-strength composite solid buoyancy materials. The overall level of research and development of domestic buoyancy materials is far behind that of foreign countries, mainly due to the lack of high-performance hollow glass microspheres. At present, microspheres generally have defects such as high density and poor strength. The root cause is the backward preparation technology of microspheres, which cannot achieve independent control of key performance parameters of microspheres (such as density and particle size).
[0003] Taking the authorized patent CN101704632B, a method for preparing high-strength and low-density hollow glass microspheres, and the authorized patent CN102320743B, aluminosilicate high-strength hollow glass microspheres and their preparation methods, as examples, the relevant patents only introduce the preparation process of hollow glass microspheres in a formulaic manner, and only give a general description of the key hollowing process. The density and particle size before and after spheroidization are only given in range values, and the corresponding general rules of the particle size and density of hollow microspheres prepared by glass powder before and after spheroidization are not given, as well as feedback to guide quantitative production. The chemical composition and method of preparing hollow glass microspheres introduced in the US patent US3365315 and the Russian patent R2059574 have a density of 0.1 to 0.7 g / cm 3 et al. also did not introduce in detail how to quantitatively achieve controllable preparation of density and particle size of hollow glass microspheres through foaming technology. Summary of the invention
[0004] The purpose of the present invention is to explore the density control technology of hollow glass microspheres and provide a preparation method of hollow glass microspheres in view of the shortcomings of poor controllability of key parameters of density and particle size of hollow glass microspheres prepared by the existing domestic glass powder method. The present invention combines theoretical deduction with actual production experience. For a given glass basic formula, the expansion ratio of the hollow glass microspheres is derived and calculated to determine the foaming dosage in the glass formula and the particle size of the glass powder before foaming. Combined with the regulation of important parameters such as the external spheroidization temperature node, the controllable preparation of the density and particle size of the hollow glass microspheres is achieved. The preparation method of the high-performance hollow glass microspheres is simple and repeatable, and is particularly suitable for providing hollow glass microspheres with corresponding parameters in deep-sea solid buoyancy materials at different depths.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for controlling the density and particle size of hollow glass microspheres, wherein the outer diameter R of the hollow glass microspheres to be prepared and the density ρ of the hollow glass microspheres to be prepared are obtained. h Under the condition of g The amount of foaming agent added is determined by the ratio.
[0007] The parameters that will be used later are as follows:
[0008] Glass powder density: ρ g , usually 2.5g / cm 3 ;
[0009] Glass powder volume: V g (cm 3 );
[0010] Glass powder radius: r g (cm);
[0011] Density of hollow glass microspheres: ρ h (g / cm 3 );
[0012] Total volume of hollow glass microspheres: V h (cm 3 );
[0013] Outer diameter of hollow glass microspheres: R (cm).
[0014] The method for determining the amount of foaming agent to be added is:
[0015] The first step is to use ρ g V g =ρ h V h , substituting the parameters into the calculation, we can get:
[0016]
[0017] The second step is to calculate the hollow glass microsphere density ρ according to the known outer diameter R of the hollow glass microsphere. h And the glass powder density ρ g Calculate R / r g ;
[0018] The third step is to use R / r g Determine the amount of foaming agent to add.
[0019] Furthermore, the radius used in the calculation is the median radius.
[0020] Furthermore, the foaming effect of the foaming agent is linearly related to the amount of the foaming agent.
[0021] Beneficial effects of the present invention:
[0022] The present invention provides a controllable preparation method of hollow glass microspheres. The control technology is universal and can achieve high controllability of the main parameters of the hollow glass microspheres in the preparation process: density, particle size and other indicators. Customized preparation can be achieved according to different application requirements of the hollow glass microspheres. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention will be further described below in conjunction with the accompanying drawings.
[0024] Figure 1 It is a schematic diagram of the hollow spheroidization process of glass powder. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] like Figure 1 As shown, hollow glass microspheres are prepared by the glass powder method. Glass powder is prepared in advance according to demand. Through high-temperature foaming control technology, the external spheroidization temperature node is controlled to trigger the foaming agent pre-added in the glass powder, so that the glass powder expands and foams to a specific particle size at a specific high temperature, thereby realizing the controllable production of hollow glass microspheres with specific density and particle size.
[0027] The specific implementation steps are as follows:
[0028] 1. Calculate the glass powder expansion ratio. Since the mass of the microspheres remains unchanged before and after foaming, ρ g V g =ρ h V h , substituting the parameters into the calculation, we can get:
[0029]
[0030] 2. Determine the particle size of the glass powder. Hollow glass microspheres are prepared by expansion and foaming of glass powder. After determining the expansion ratio, the particle size of the glass powder before spheroidization can be reversed.
[0031] 3. The amount of foaming agent added in the formula. The foaming effect of the foaming agent is linearly related to the amount of the foaming agent. The amount of foaming agent added can be determined based on the expansion ratio.
[0032] The density of the glass was 0.15 g / cm 3, take hollow glass microspheres with a median particle size of D50 = 60 μm as an example. The Tm temperature of glass is 1400-1490°C. Substitute into the formula to calculate R / r g =2.55, indicating that the diameter of the finished hollow glass microspheres has expanded by 2.55 times relative to the diameter of the raw glass powder. At this time, according to production experience, 1% of foaming agent can make the diameter of the glass powder expand by 1 time, so the amount of foaming agent added is 2.55%; the particle size D50 of the glass powder before spheroidization should be 60 / 2.55=23.5μm.
[0033] In summary, if we want to use glass formula D to prepare a glass with a density of 0.15 g / cm 3 , hollow glass microspheres with a median particle size of d50 = 60μm, only need to add 2.55% of foaming agent to the glass formula D, the particle size D50 of the glass powder before spheroidization is controlled at about 23.5μm, and the spheroidization temperature is controlled between 1400-1490℃ to achieve.
[0034] Example 1
[0035] Recipe A
[0036]
[0037]
[0038] A-1. Preparation of hollow glass microspheres with a density of 0.15 g / cm using formula A 3 , median particle size D50 = 60 μm, glass Tm temperature 1441-1462°C.
[0039] Substituting into formula (1) to determine the glass powder expansion ratio, we calculated R / rg = 2.55, which means that the diameter of the finished hollow glass microspheres has expanded by 2.55 times relative to the diameter of the raw glass powder. At this time, according to production experience, 1% of foaming agent can make the glass powder diameter expand by 1 times, so the amount of foaming agent added is 2.55%; the particle size D50 of the glass powder before spheroidization should be 60 / 2.55 = 23.5μm.
[0040] In summary, if we want to use glass formula A to prepare a glass with a density of 0.15 g / cm 3 , hollow glass microspheres with a median particle size of d50 = 60μm. It can be achieved by adding 2.55% of foaming agent to glass formula A, controlling the particle size D50 of the glass powder before spheroidization to about 23.5μm, and controlling the spheroidization temperature between 1441-1462℃. The measured strength of the product is 3.45MPa, and the yield rate is 85%.
[0041] A-2. Similarly, hollow glass microspheres with a density of 0.38 g / cm were prepared using formula A. 3 , median particle size D50 = 38 μm, glass Tm temperature 1441-1462°C.
[0042] Substituting into formula (1) to determine the glass powder expansion ratio, we calculated R / rg = 1.87, which means that the diameter of the finished hollow glass microspheres has expanded by 1.87 times relative to the diameter of the raw glass powder. At this time, according to production experience, 1% of the foaming agent can make the glass powder diameter expand by 1 times, so the amount of foaming agent added is 1.87%; the particle size D50 of the glass powder before spheroidization should be 38 / 1.87 = 20.3μm.
[0043] In summary, if we want to use glass formula A to prepare a glass with a density of 0.38 g / cm 3 , hollow glass microspheres with a median particle size of d50 = 38μm. It can be achieved by adding 1.87% of foaming agent to glass formula A, controlling the particle size D50 of the glass powder before spheroidization to about 20.3μm, and controlling the spheroidization temperature between 1441-1462℃. The measured strength of the product is 22.5MPa, and the yield rate is 35%.
[0044] A-3 is similar to the hollow glass microspheres prepared by formula A with a density of 0.45 g / cm 3 , median particle size D50 = 20 μm, glass Tm temperature 1441-1462°C.
[0045] Substituting into formula (3) to determine the glass powder expansion ratio, we calculated R / rg = 1.77, which means that the diameter of the hollow glass microspheres has expanded by 1.77 times relative to the diameter of the raw glass powder. Therefore, the amount of foaming agent added is 1.77%. The particle size D50 of the glass powder before spheroidization should be 20 / 1.77 = 11.3 μm.
[0046] In summary, if we want to use glass formula A to prepare a glass with a density of 0.45 g / cm 3 , hollow glass microspheres with a median particle size of d50 = 20μm. It can be achieved by adding 1.77% of foaming agent to glass formula A, controlling the particle size D50 of the glass powder before spheroidization to about 11.3μm, and controlling the spheroidization temperature between 1441-1462℃. The measured strength of the product is 37.8MPa, and the yield rate is 28%.
[0047]
[0048] Example 2
[0049] Recipe B:
[0050] Serial number <![CDATA[SiO 2 ]]> <![CDATA[Na 2 The]]> CaO <![CDATA[B 2 THE 3 ]]> <![CDATA[Li 2 The]]> ZnO <![CDATA[Al 2 THE 3 ]]> E(GP) <![CDATA[T m (℃)]]> B 68 7.5 9 9 2 1.5 3 82.96 1498-1537
[0051] B-1 hollow glass microspheres prepared with formula B, density 0.15 g / cm 3 , median particle size D50 = 60 μm, glass Tm temperature 1498-1537 °C.
[0052] Substituting into formula (1) to determine the glass powder expansion ratio, we calculated R / rg = 2.55, which means that the diameter of the finished hollow glass microspheres has expanded by 2.55 times relative to the diameter of the raw glass powder. At this time, according to production experience, 1% of foaming agent can make the glass powder diameter expand by 1 times, so the amount of foaming agent added is 2.55%; the particle size D50 of the glass powder before spheroidization should be 60 / 2.55 = 23.5μm.
[0053] In summary, if we want to use glass formula B to prepare a glass with a density of 0.15 g / cm 3 , hollow glass microspheres with a median particle size of d50 = 60μm. It can be achieved by adding 2.55% of foaming agent to glass formula B, controlling the particle size D50 of the glass powder before spheroidization to about 23.5μm, and controlling the spheroidization temperature between 1498-1537℃. The measured strength of the product is 3.74MPa, and the yield rate is 21%.
[0054] B-2 is similar to the hollow glass microspheres prepared by formula B. The density is 0.38 g / cm 3 , median particle size D50 = 38 μm, glass Tm temperature 1498-1537 °C.
[0055] Substituting into formula (1) to determine the glass powder expansion ratio, we calculated R / rg = 1.87, which means that the diameter of the finished hollow glass microspheres has expanded by 1.87 times relative to the diameter of the raw glass powder. At this time, according to production experience, 1% of the foaming agent can make the glass powder diameter expand by 1 times, so the amount of foaming agent added is 1.87%; the particle size D50 of the glass powder before spheroidization should be 38 / 1.87 = 20.3μm.
[0056] In summary, if we want to use glass formula B to prepare a glass with a density of 0.38 g / cm 3 , hollow glass microspheres with a median particle size of d50 = 38μm. It can be achieved by adding 1.87% of foaming agent to glass formula B, controlling the particle size D50 of the glass powder before spheroidization to about 20.3μm, and controlling the spheroidization temperature between 1498-1537℃. The measured strength of the product is 37.9MPa, and the yield rate is 75%.
[0057] B-3 is similar to the hollow glass microspheres prepared with formula B. The density is 0.45 g / cm 3 , median particle size D50 = 20 μm, glass Tm temperature 1498-1537°C.
[0058] Substituting into formula (1) to determine the glass powder expansion ratio, we calculated R / rg = 1.77, which means that the diameter of the hollow glass microspheres has expanded by 1.77 times relative to the diameter of the raw glass powder. Therefore, the amount of foaming agent added is 1.77%. The particle size D50 of the glass powder before spheroidization should be 20 / 1.77 = 11.3 μm.
[0059] In summary, if we want to use glass formula B to prepare a glass with a density of 0.45 g / cm 3 , hollow glass microspheres with a median particle size of d50 = 20μm. It can be achieved by adding 1.77% of foaming agent to glass formula B, controlling the particle size D50 of the glass powder before spheroidization to about 11.3μm, and controlling the spheroidization temperature between 1498-1537℃. The measured strength of the product is 47.8MPa, and the yield rate is 31%.
[0060]
[0061] Example 3
[0062] Recipe C
[0063] Serial number <![CDATA[SiO 2 ]]> <![CDATA[Na 2 The]]> CaO <![CDATA[B 2 THE 3 ]]> <![CDATA[Li 2 The]]> ZnO <![CDATA[Al 2 THE 3 ]]> E(GP) <![CDATA[T m (℃)]]> C 70 6 9 12 0.5 1 1.5 86.01 1469-1507
[0064] C-1 Hollow glass microspheres prepared with formula C, density 0.15 g / cm 3 , median particle size D50 = 60 μm, glass Tm temperature 1469-1507°C.
[0065] Substituting into formula (1) to determine the glass powder expansion ratio, we calculated R / rg = 2.55, which means that the diameter of the finished hollow glass microspheres has expanded by 2.55 times relative to the diameter of the raw glass powder. At this time, according to production experience, 1% of foaming agent can make the glass powder diameter expand by 1 times, so the amount of foaming agent added is 2.55%; the particle size D50 of the glass powder before spheroidization should be 60 / 2.55 = 23.5μm.
[0066] In summary, if we want to use glass formula C to prepare a glass with a density of 0.15 g / cm 3 , hollow glass microspheres with a median particle size of d50 = 60μm. It can be achieved by adding 2.55% of foaming agent to glass formula C, controlling the particle size D50 of the glass powder before spheroidization to about 23.5μm, and controlling the spheroidization temperature between 1469-1507℃. The measured strength of the product is 3.81MPa, and the yield rate is 18%.
[0067] C-2 is similar to the hollow glass microspheres prepared with formula C. The density is 0.38 g / cm 3 , median particle size D50 = 38 μm, glass Tm temperature 1469-1507 °C.
[0068] Substituting into formula (1) to determine the glass powder expansion ratio, we calculated R / rg = 1.87, which means that the diameter of the finished hollow glass microspheres has expanded by 1.87 times relative to the diameter of the raw glass powder. At this time, according to production experience, 1% of the foaming agent can make the glass powder diameter expand by 1 times, so the amount of foaming agent added is 1.87%; the particle size D50 of the glass powder before spheroidization should be 38 / 1.87 = 20.3μm.
[0069] In summary, if we want to use glass formula C to prepare a glass with a density of 0.38 g / cm 3 , hollow glass microspheres with a median particle size of d50 = 38μm. It can be achieved by adding 1.87% of foaming agent to glass formula C, controlling the particle size D50 of the glass powder before spheroidization to about 20.3μm, and controlling the spheroidization temperature between 1469-1507℃. The measured strength of the product is 38.2MPa, and the yield rate is 21%.
[0070] C-3 is similar to the hollow glass microspheres prepared with formula C. The density is 0.45 g / cm 3 , median particle size D50 = 20 μm, glass Tm temperature 1469-1507°C.
[0071] Substituting into formula (1) to determine the glass powder expansion ratio, we calculated R / rg = 1.77, which means that the diameter of the hollow glass microspheres has expanded by 1.77 times relative to the diameter of the raw glass powder. Therefore, the amount of foaming agent added is 1.77%. The particle size D50 of the glass powder before spheroidization should be 20 / 1.77 = 11.3 μm.
[0072] In summary, if we want to use glass formula B to prepare a glass with a density of 0.45 g / cm 3 , hollow glass microspheres with a median particle size of d50 = 20μm. It can be achieved by adding 1.77% of foaming agent to glass formula C, controlling the particle size D50 of the glass powder before spheroidization to about 11.3μm, and controlling the spheroidization temperature between 1469-1507℃. The measured strength of the product is 55.2MPa, and the yield rate is 62%.
[0073]
[0074] The above embodiments fully illustrate that the present invention can realize the precise and controllable preparation and forming of hollow glass microspheres with different densities / particle sizes under the same formula / different formulas by controlling the crushing particle size of the glass powder, the amount of foaming agent added and the spheroidization foaming temperature, thereby giving full play to the advantages of the glass powder preparation process.
[0075] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for controlling density and particle size of hollow glass microspheres, characterized in that: After obtaining the outer diameter R of the hollow glass microspheres to be prepared and the density ρ of the hollow glass microspheres h Under the condition of g The amount of foaming agent added is determined by the ratio.
2. The method for controlling density and particle size of hollow glass microspheres according to claim 1, characterized in that: The method for determining the amount of foaming agent to be added is: The first step is to use ρ g V g =ρ h V h , substituting the parameters into the calculation, we can get: Glass powder density: ρ g ; Glass powder volume: V g ; Glass powder radius: r g ; Density of hollow glass microspheres: ρ h ; Total volume of hollow glass microspheres: V h ;Outer diameter of hollow glass microspheres: R; The second step is to calculate the hollow glass microsphere density ρ according to the known outer diameter R of the hollow glass microsphere. h And the glass powder density ρ g Calculate R / r g ; The third step is to use R / r g Determine the amount of foaming agent to add.
3. The method for controlling density and particle size of hollow glass microspheres according to claim 2, characterized in that: The radius used in the calculation is the median radius.
4. The method for controlling density and particle size of hollow glass microspheres according to claim 2, characterized in that: The foaming effect of the foaming agent is linearly related to the amount of the foaming agent.
Citation Information
Patent Citations
Method for preparing microporous foam glass by use of waste glass
CN103553343A
Low-density solid buoyancy material suitable for deep sea and preparation method thereof
CN113683862A
Method for controlling particle size of hollow glass beads according to design requirements in production
CN114907017A