Aluminosilicate glass, preparation method thereof and cover plate glass
Through atomization treatment and crystallization reaction to form high volume density block materials, combined with casting molding and annealing treatment, the problem of high melting temperature of aluminosilicate glass is solved, the melting temperature and raw material scattering are reduced, and the quality of the finished product is improved. efficiency and physical and chemical properties.
Patent Information
- Application Number
- CN202411030418.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-29
AI Technical Summary
The melting temperature of aluminosilicate glass is high, which leads to increased difficulty and fuel consumption during the preparation process, and it is difficult for traditional methods to ensure the composition uniformity of the finished product and the reduction of bubble defects.
Atomization treatment is used to mix the clarifier, binder and water to form an atomized material and mix it with the powder. The block material with high volume density is formed through crystallization reaction and tableting process, and is poured, molded and annealed during the melting process. Processing, lowering the melting temperature, reducing the scattering of raw materials, ensuring the composition uniformity of the finished product and reducing bubble defects.
It effectively reduces the melting temperature of aluminosilicate glass, increases the melting rate and heat conduction rate, reduces the scattering of raw materials, improves the yield and physical and chemical properties of the finished product, and has the advantages of stable glass composition and low cost.
Smart Images

Figure CN118851566A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of glass, and in particular to an aluminosilicate glass and a preparation method thereof and a cover glass. Background Art
[0002] Glass is widely used in many fields, such as door and window glass in the construction industry, window glass and windshield of vehicles, cover glass of electronic touch devices, etc. With the development of mobile platforms and the advancement of display technologies such as smart phones, tablet computers, digital cameras, and smart TVs, ultra-thin electronic glass has attracted widespread attention due to its ultra-thin and ultra-light characteristics, and has been rapidly developed and widely used.
[0003] Before ultra-thin electronic glass is made into cover glass for display devices, it usually needs to be chemically tempered to enhance its mechanical strength, thermal stability and safety, thereby effectively preventing the screen from being damaged by impact or scratches. For aluminosilicate glass, increasing the Al2O3 content is beneficial to improving its intrinsic mechanical strength and chemical tempering performance, but at the same time it will also cause its melting temperature to be high, making it difficult to melt and process. Summary of the invention
[0004] Based on this, it is necessary to provide an aluminosilicate glass and a preparation method thereof and a cover glass to solve the problem that the melting temperature of traditional aluminosilicate glass is relatively high.
[0005] The above-mentioned purpose of the present application is achieved through the following technical solutions:
[0006] In a first aspect of the present application, a method for preparing aluminosilicate glass is provided, comprising the following steps:
[0007] Mixing a clarifier, a binder and water, performing atomization treatment to prepare an atomized material, and mixing the remaining raw materials of the aluminosilicate glass to prepare a powder material;
[0008] Mixing the atomized material and the powder material to prepare a batch material;
[0009] Allowing the batch material to undergo a crystallization reaction to prepare a crystallized material;
[0010] The crystallized material is tableted to prepare a block material;
[0011] Performing melting treatment, molding treatment and annealing treatment on the block material to prepare the aluminosilicate glass;
[0012] Wherein, the binder includes one or more of sodium silicate, sodium hydroxide and sodium carbonate;
[0013] The masses of the clarifier, the binder, the water and the powder are a, b, c and d respectively, satisfying: a:b:c:(a+d)=(0.1~0.7):(2~9):(1~8):100.
[0014] In one embodiment, the aluminosilicate glass comprises the following components in mass fractions:
[0015] .
[0016] In one embodiment, the clarifier includes one or more of tin oxide, antimony oxide, cerium oxide, sodium sulfate, barium sulfate, calcium sulfate, sodium nitrate, ammonium nitrate, sodium chloride, ammonium chloride, calcium fluoride and sodium fluorosilicate.
[0017] In one embodiment, the atomization treatment methods independently include one or more of high-pressure spray gun atomization, ultrasonic atomization and rotary atomization.
[0018] In one embodiment, the spray gun pressure of the high-pressure spray gun atomization method is 0.3MPa~0.8MPa.
[0019] In one embodiment, the spray flow rate of the high-pressure spray gun atomization method is 0.5slm~2slm.
[0020] In one embodiment, the atomization time of the atomization treatment is 10 min to 20 min.
[0021] In one embodiment, subjecting the batch material to a crystallization reaction comprises the following steps:
[0022] The batch material is allowed to stand at room temperature for 4 h to 24 h.
[0023] In one embodiment, the crystallized material is tableted, comprising the following steps: placing the crystallized material in a tableting mold, applying a pressure of 2t to 8t, so that the bulk density of the block material is ≥1.9g / cm 3 .
[0024] In one embodiment, the melting process includes the following steps: keeping warm at 1580°C~1630°C for 4h~8h.
[0025] In one embodiment, the molding process includes a casting molding method.
[0026] In one of the embodiments, the annealing treatment includes the following steps: cooling from 1000°C to 700°C to room temperature, and the cooling time is ≥12h.
[0027] In one of the embodiments, after the annealing treatment, the following step is further included: placing the aluminosilicate glass in molten salt and chemically toughening it at 390° C. to 430° C. for 3 h to 8 h.
[0028] In a second aspect of the present application, an aluminosilicate glass is provided, which is prepared by the aluminosilicate glass preparation method as described above.
[0029] In one embodiment, the melting temperature of the aluminosilicate glass is 1580°C to 1630°C.
[0030] In one embodiment, the softening temperature of the aluminosilicate glass is 700°C to 750°C.
[0031] In one embodiment, the linear expansion coefficient of the aluminosilicate glass in the range of 30°C to 300°C is 90×10 -7 / ℃~100×10 -7 / ℃.
[0032] In one of the embodiments, the surface compressive stress of the aluminosilicate glass is 620 MPa~900 MPa.
[0033] In one of the embodiments, the stress layer depth of the aluminosilicate glass is 28 μm to 45 μm.
[0034] In a second aspect of the present application, a cover glass is provided, which is made of the aluminosilicate glass as described above.
[0035] This application has at least the following beneficial effects:
[0036] The present application first atomizes a mixture of a clarifier, a binder and water to form an atomized material through atomization treatment, and then mixes the atomized material with a powder material to promote the clarifier and the binder to be highly evenly dispersed in the batch material. The binder includes one or more of sodium silicate, sodium hydroxide and sodium carbonate, which will fully react with the remaining raw materials and be converted into a crystalline compound during the crystallization reaction, making the bonding effect stronger, which is conducive to the tableting of the crystallized material into blocks, thereby obtaining a block material with a high volume density. The increase in volume density can increase the unit melting rate and heat conduction rate, thereby significantly reducing the melting temperature, and then reducing the difficulty of the melting process and fuel consumption.
[0037] At the same time, melting the block material with high volume density can not only reduce the flying of raw materials in the melting furnace and ensure the uniformity of the composition of the finished glass, but also inhibit the erosion of the melting furnace by the flying materials, effectively extending the service life of the melting furnace. In addition, the uniform mixing and close contact between the clarifier and the other raw materials can promote the efficient removal of bubbles in the molten glass liquid, ensuring that the bubble defects and crystallization stone defects of the finished glass are very few or even absent, and the finished product yield is high. Therefore, the preparation method of aluminosilicate glass provided in the present application can effectively improve the uniformity and melting rate of the mixing, reduce the melting temperature, reduce the flying of raw materials, and has the advantages of stable glass composition, good physical and chemical properties, high finished product yield and low cost, which is conducive to industrial mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.
[0039] Figure 1 Schematic diagram of a conventional method for preparing aluminosilicate glass;
[0040] Figure 2 Schematic diagram of a process for preparing aluminosilicate glass in one embodiment. DETAILED DESCRIPTION
[0041] In order to facilitate the understanding of the present application, the present application is further described in detail below in conjunction with specific embodiments. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0043] In the present application, the meaning of "and / or" includes any and all combinations of one or more related listed items. "At least one" means more than one, such as one, two and more than two. "Multiple" or "several" means at least two, such as two, three, etc., and "multi-layer" means at least two layers, such as two layers, three layers, etc., unless otherwise clearly and specifically defined. In the description of the present application, "several" means at least one, such as one, two, etc., unless otherwise clearly and specifically defined.
[0044] When a numerical range is disclosed in this application, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed in this application should be understood to include any and all subranges included therein.
[0045] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0046] In this application, "above" or "below" includes the number itself. For example, "1 below" includes 1.
[0047] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0048] In the present application, room temperature refers to indoor temperature, normal temperature or general temperature. Generally speaking, the range of room temperature can be any one of the following temperature intervals: 23°C ± 2°C, 25°C ± 5°C or 20°C ± 5°C.
[0049] the term
[0050] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0051] Melting Temperature (T m ): The melting point of glass refers to the temperature at which glass completely changes from solid to liquid at high temperature.
[0052] Softening Temperature (T s): Also known as the softening point, the softening temperature of glass refers to the temperature at which glass begins to soften and flow at high temperatures. The softening temperature of glass is usually between its glass transition temperature (T g ) and the melting temperature.
[0053] Coefficient of Thermal Expansion (CTE): usually refers to the linear expansion coefficient. The linear expansion coefficient refers to the change in the length value of a material due to a unit temperature change. It is usually expressed as the linear expansion coefficient in a certain temperature range, with the unit of 1 / ℃ or 1 / K.
[0054] Glass can be classified into soda-lime glass, lead silicate glass, aluminosilicate glass, borosilicate glass and quartz glass according to its chemical composition. Ordinary soda-lime glass has small surface compressive stress (Compressed Stress, CS) and stress layer depth (DOL) after chemical tempering, and cannot effectively protect the screen. Aluminosilicate glass has a high Al2O3 content, and its intrinsic mechanical strength and chemical tempering performance are significantly better than soda-lime glass. After chemical tempering, medium-aluminum glass has a low stress layer depth and cannot be used in scenes with high requirements for mechanical properties. High-aluminum glass (usually Al2O3 content ≥ 6wt.%) has excellent impact and scratch resistance after chemical tempering.
[0055] See also Figure 1 , which is a schematic diagram of a conventional method for preparing aluminosilicate glass. The conventional method for preparing aluminosilicate glass comprises the following steps:
[0056] S110: Mixing all raw materials of aluminosilicate glass to obtain a batch material;
[0057] S120: performing melting treatment, molding treatment and annealing treatment on the batch materials to obtain aluminosilicate glass.
[0058] However, through simple mixing treatment, the mixing uniformity of the batch is poor and the volume density is low, resulting in low unit melting rate and heat conduction efficiency, which significantly increases the melting temperature. In addition, for aluminosilicate glass, although the increase in Al2O3 content is beneficial to improve its intrinsic mechanical strength and chemical tempering performance, it will also significantly increase its melting temperature, making the melting difficulty further increased. Therefore, it is necessary to optimize the preparation process of aluminosilicate glass to reduce the melting temperature of aluminosilicate glass, especially the melting temperature of high-aluminum glass, so as to improve the melting efficiency and reduce the melting difficulty while improving the physical and chemical properties of aluminosilicate glass.
[0059] Based on this, in the first aspect of the present application, a method for preparing aluminosilicate glass is provided.
[0060] See also Figure 2 , which is a schematic flow chart of a method for preparing aluminosilicate glass in an embodiment. In some embodiments, the method for preparing aluminosilicate glass comprises the following steps:
[0061] S210: mixing a clarifier, a binder and water, performing atomization treatment to prepare an atomized material, and mixing the remaining raw materials of the aluminosilicate glass to prepare a powder material;
[0062] S220: Mixing atomized material and powder material to prepare a batch material;
[0063] S230: subjecting the batch material to a crystallization reaction to prepare a crystal material;
[0064] S240: tabletting the crystallized material to prepare a block material;
[0065] S250: performing melting treatment, forming treatment and annealing treatment on the block material to prepare aluminosilicate glass;
[0066] Wherein, the binder includes one or more of sodium silicate, sodium hydroxide and sodium carbonate;
[0067] The masses of clarifier, binder, water and powder are a, b, c and d respectively, satisfying: a:b:c:(a+d)=(0.1~0.7):(2~9):(1~8):100.
[0068] The present application first atomizes a mixture of a clarifier, a binder and water to form an atomized material through atomization treatment, and then mixes the atomized material with a powder material to promote the clarifier and the binder to be highly evenly dispersed in the batch material. The binder includes one or more of sodium silicate, sodium hydroxide and sodium carbonate, which will fully react with the remaining raw materials and be converted into a crystalline compound during the crystallization reaction, making the bonding effect stronger, which is conducive to the tableting of the crystallized material into blocks, thereby obtaining a block material with a high volume density. The increase in volume density can increase the unit melting rate and heat conduction rate, thereby significantly reducing the melting temperature, and then reducing the difficulty of the melting process and fuel consumption.
[0069] At the same time, melting the block material with high volume density can not only reduce the flying of raw materials in the melting furnace and ensure the uniformity of the composition of the finished glass, but also inhibit the erosion of the melting furnace by the flying materials, effectively extending the service life of the melting furnace. In addition, the uniform mixing and close contact between the clarifier and the other raw materials can promote the efficient removal of bubbles in the molten glass liquid, ensuring that the bubble defects and crystallization stone defects of the finished glass are very few or even absent, and the finished product yield is high. Therefore, the preparation method of aluminosilicate glass provided in the present application can effectively improve the uniformity and melting rate of the mixing, reduce the melting temperature, reduce the flying of raw materials, and has the advantages of stable glass composition, good physical and chemical properties, high finished product yield and low cost, which is conducive to industrial mass production.
[0070] As an example, the binder can be selected from one of sodium silicate (Na2SiO3), sodium hydroxide (NaOH) and sodium carbonate (Na2CO3), and can also be selected from one of the following combinations: Na2SiO3 and NaOH; Na2SiO3; NaOH and Na2CO3; Na2SiO3 and Na2CO3; and Na2SiO3, NaOH and Na2CO3.
[0071] As an example, the water can be one or more of tap water, deionized water, distilled water, reverse osmosis water, pure water and ultrapure water. Using tap water is conducive to reducing the cost, and using deionized water, distilled water or pure water is conducive to improving the quality of the finished glass.
[0072] As an example, the ratio of the mass of the clarifier to the total mass of the clarifier and the powder may be 0.1:100, 0.2:100, 0.3:100, 0.4:100, 0.5:100, 0.6:100 or 0.7:100.
[0073] As an example, the ratio of the mass of the binder to the total mass of the clarifier and the powder may be 2:100, 3:100, 4:100, 5:100, 6:100, 7:100, 8:100 or 9:100.
[0074] As an example, the ratio of the mass of water to the total mass of the clarifier and the powder may be 1:100, 2:100, 3:100, 4:100, 5:100, 6:100, 7:100 or 8:100.
[0075] Optionally, the aluminosilicate glass includes the following components in mass fractions:
[0076] .
[0077] Traditional high-aluminum glass also has a high softening temperature and linear expansion coefficient. If the softening temperature is too high, high-aluminum glass is difficult to bend plastically, which is not conducive to the preparation of curved glass cover plates. Using a hot bending mold to match high-aluminum glass with a high linear expansion coefficient will cause problems such as high energy consumption for hot bending plasticity, deep mold impression of hot-bent products, and short service life of hot bending molds. Therefore, in one embodiment of the present application, the content of each component of aluminosilicate glass is optimized to reduce its softening temperature and linear expansion coefficient while obtaining higher mechanical strength and strengthening performance.
[0078] As an example, the mass fraction of SiO2 in the aluminosilicate glass can be 58%, 58.5%, 59%, 59.5%, 60%, 60.5%, 61%, 61.5%, 62%, 62.5%, 63%, 63.5%, 64%, 64.5%, 65%, 65.5% or 66%.
[0079] As an example, the mass fraction of Al2O3 in the aluminosilicate glass can be 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5% or 15%.
[0080] As an example, the mass fraction of Na2O in the aluminosilicate glass may be 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16% or 16.5%.
[0081] As an example, the mass fraction of K2O in the aluminosilicate glass may be 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5% or 8%.
[0082] As an example, the mass fraction of MgO in the aluminosilicate glass may be 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5% or 7%.
[0083] As an example, the mass fraction of ZrO2 in the aluminosilicate glass can be 0.2%, 0.4%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.6%, 1.8% or 2%.
[0084] As an example, the mass fraction of B2O3 in the aluminosilicate glass can be 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%.
[0085] As an example, the mass fraction of the fining agent in the aluminosilicate glass may be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6% or 0.7%.
[0086] Optionally, the raw materials of the aluminosilicate glass include a SiO2 source, an Al2O3 source, a Na2O source, a K2O source, a MgO source, a ZrO2 source, a B2O3 source and a clarifier.
[0087] Optionally, the SiO2 source includes one or more of quartz sand (SiO2) and silicates, wherein the silicates include one or more of sodium silicate (Na2SiO3), potassium silicate (K2SiO3), aluminum silicate (Al2O3·SiO2) and calcium silicate (CaSiO3).
[0088] Optionally, the Na2O source includes one or more of sodium silicate (Na2SiO3), sodium hydroxide (NaOH), sodium carbonate (Na2CO3) and sodium bicarbonate (NaHCO3).
[0089] It can be understood that Na2SiO3 in the binder can be used as a SiO2 source and a Na2O source, and NaOH and Na2CO3 can be used as Na2O sources. Therefore, when calculating the amount of SiO2 source and Na2O source, the SiO2 and Na2O introduced in the binder should be deducted. In order to accurately control the amount of SiO2 source, Na2O source and binder, in some specific examples, quartz sand is selected as the SiO2 source, Na2CO3 is selected as the Na2O source, and Na2SiO3 and / or NaOH are selected as the binder. In some other specific examples, part of Na2CO3 can also be used as a Na2O source and formed into a powder through mixing treatment, and part of Na2CO3 can be used as a binder and formed into an atomized material through atomization treatment. The same is true for Na2SiO3 and NaOH, which will not be repeated.
[0090] Optionally, the Al2O3 source includes one or more of aluminum oxide (Al2O3) and aluminum hydroxide (Al(OH)3), and may further be Al2O3.
[0091] Optionally, the K2O source includes one or more of potassium carbonate (K2CO3) and potassium bicarbonate (KHCO3), and further optionally K2CO3.
[0092] Optionally, the MgO source includes one or more of magnesium oxide (MgO) and magnesium carbonate ((MgCO 3 )), and further optionally is MgO.
[0093] Optionally, the ZrO 2 source includes one or more of zirconium oxide (ZrO 2 ) and zirconium carbonate (Zr(CO 3 ) 2 ), and may further be ZrO 2 .
[0094] Optionally, the B2O3 source includes one or more of borax (Na2B4O7) and boric acid (H3BO3), and may further be H3BO3.
[0095] Optionally, the clarifier includes one or more of tin oxide (SnO2), antimony oxide (Sb2O3), cerium oxide (CeO2), sodium sulfate (Na2SO4), barium sulfate (BaSO4), calcium sulfate (CaSO4), sodium nitrate (NaNO3), ammonium nitrate (NH4NO3), sodium chloride (NaCl), ammonium chloride (NH4Cl), calcium fluoride (CaF2) and sodium fluorosilicate (Na2SiF6), and may further be one or more of SnO2, CeO2 and NaNO3.
[0096] Meanwhile, the raw materials of each component of the aluminosilicate glass may be a compound containing water of crystallization or a compound not containing water of crystallization. For example, borax may be sodium borate decahydrate (Na2B4O7·10H2O), sodium borate pentahydrate (Na2B4O7·5H2O) or anhydrous sodium borate (Na2B4O7). In order to accurately control the amount of water used in step S210, the raw materials of the aluminosilicate glass may further be selected to be a compound not containing water of crystallization.
[0097] Optionally, the atomization method includes one or more of high-pressure spray gun atomization, ultrasonic atomization and rotary atomization, and high-pressure spray gun atomization can be further selected.
[0098] Optionally, the spray gun pressure of the high-pressure spray gun atomization method is 0.3 MPa to 0.8 MPa, for example, 0.3 MPa, 0.35 MPa, 0.4 MPa, 0.45 MPa, 0.5 MPa, 0.55 MPa, 0.6 MPa, 0.65 MPa, 0.7 MPa, 0.75 MPa or 0.8 MPa.
[0099] Optionally, the spray flow rate of the high-pressure spray gun atomization method is 0.5slm to 2slm, such as 0.5slm, 0.6slm, 0.7slm, 0.8slm, 0.9slm, 1slm, 1.1slm, 1.2slm, 1.3slm, 1.4slm, 1.5slm, 1.6slm, 1.7slm, 1.8slm, 1.9slm or 2slm. Wherein, slm is the abbreviation of standard litre per minute, indicating a flow rate of 1L / min under standard conditions.
[0100] Optionally, the atomization time of the atomization treatment is 5 min to 15 min, for example, 5 min, 7 min, 9 min, 11 min, 13 min or 15 min.
[0101] Optionally, the remaining raw materials of the mixed aluminosilicate glass include the following steps: placing the remaining raw materials of the aluminosilicate glass in a mixer and mixing for 3 min to 15 min, such as 3 min, 5 min, 7 min, 9 min, 11 min, 13 min or 15 min.
[0102] Optionally, mixing the atomized material and the powder material includes the following steps: placing the atomized material and the powder material in a mixer and mixing for 2 min to 8 min.
[0103] Optionally, subjecting the batch material to a crystallization reaction includes the following steps: allowing the batch material to stand at room temperature for 8 h to 48 h.
[0104] It can be understood that during the crystallization reaction, the binder, water and the remaining raw materials will fully react, significantly enhancing the bonding effect, which is beneficial to forming a bulk material with a high bulk density through tabletting. Taking Na2CO3 as an example, Na2CO3 in the batch material will continuously undergo a hydration reaction during standing, generating a hydration product Na2CO3·nH2O (1 < n ≤ 10), and crystalline hydrated sodium carbonate will be precipitated through crystallization. The hydration product of Na2CO3 changes with temperature. During the hydration process, water molecules in the batch material will be arranged directionally around Na2CO3 molecules. Subsequently, the crystal volume of hydrated sodium carbonate expands, the hydration film covering the surface of Na2CO3 becomes thinner, causing an increase in surface tension, continuously enhancing the bonding effect of the binder until all the hydration products of sodium carbonate are converted into Na2CO3·10H2O. Similarly, Na2SiO3 will also be gradually converted into Na2SiO3·10H2O during the crystallization reaction. The hydrate of NaOH is usually monohydrate NaOH·H2O. At the same time, NaOH will react with CO2 in the air and be converted into Na2CO3, and further hydrated into Na2CO3·nH2O.
[0105] As an example, the reaction temperature of the crystallization reaction can be 15 °C to 35 °C, such as 15 °C, 16 °C, 18 °C, 20 °C, 22 °C, 24 °C, 25 °C, 26 °C, 28 °C, 30 °C, 32 °C, 34 °C or 35 °C.
[0106] As an example, the standing time of the crystallization reaction can be 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h, 26 h, 28 h, 30 h, 32 h, 34 h, 36 h, 38 h, 40 h, 42 h, 44 h, 46 h or 48 h.
[0107] Optionally, subjecting the crystallized material to tabletting treatment includes the following steps: placing the crystallized material in a tabletting mold and applying a pressure of 2 tons (t) to 8 tons (t) to make the bulk density of the bulk material ≥ 1.9 g / cm 3 .
[0108] It can be understood that through the strong bonding effect inside and the high pressure effect outside, the stacking gaps between the various substances of the crystallized material are gradually reduced, thereby obtaining a volume density ≥1.9g / cm 3 of block materials. Thanks to the significant increase in volume density, the heat conduction rate in the block materials is faster, and the unit melting rate is also significantly improved, thereby effectively reducing the melting temperature. In addition, when the block materials after tableting are sent to the kiln for melting, the flying material phenomenon is effectively suppressed, especially the volatilization rate of highly corrosive components such as B2O3 is also greatly reduced. On the one hand, it can ensure the uniformity of the composition of the finished glass, and on the other hand, it suppresses the erosion of the melting furnace by flying materials. The service life of the kiln grid body can be increased by 3 to 4 times, the service life is extended by 3 to 4 years, and the service life of the kiln crown is increased by 2 years.
[0109] As an example, the bulk density of the block may be 1.90 g / cm 3 、1.92g / cm 3 , 1.94g / cm 3 , 1.96g / cm 3 、1.98g / cm 3 , 2.00g / cm 3 , 2.02g / cm 3 , 2.04g / cm 3 , 2.06g / cm 3 , 2.08g / cm 3 , 2.10g / cm 3 , 2.12g / cm 3 , 2.14g / cm 3 , 2.16g / cm 3 , 2.18g / cm 3 or 2.20g / cm 3 , further optional to 1.98g / cm 3 ~2.15g / cm 3 .
[0110] As an example, the pressure applied to the tableting mold can be 2t, 2.5t, 3t, 3.5t, 4t, 4.5t, 4t, 5.5t, 6t, 6.5t, 7t, 7.5t or 8t.
[0111] It is understood that the tableting process is carried out at room temperature, which can be 15°C to 30°C. At the same time, there are no special restrictions on the tableting time, shape, size and material of the tableting mold, as long as the bulk density of the block material can reach 1.9g / cm 3In some specific examples, the tableting process takes 3s to 10s, the tableting mold is circular, the inner diameter of the cavity is 10mm, the height is 8mm, and the material includes but is not limited to: wear-resistant stainless steel, stainless steel with ceramic coating, and ceramic.
[0112] Optionally, the melting treatment includes the following steps: keeping warm at 1580°C~1630°C for 4h~8h.
[0113] As an example, the melting temperature of the melting process may be 1580°C, 1585°C, 1590°C, 1595°C, 1600°C, 1605°C, 1610°C, 1615°C, 1620°C, 1625°C, or 1630°C.
[0114] As an example, the holding time of the melting process can be 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h or 8h.
[0115] Optionally, the molding process includes a casting molding method.
[0116] Optionally, the casting method includes the following steps: cooling the molten glass to 1500°C-1550°C, and casting it into a forming mold at room temperature and pressure. The shape, size and material of the forming mold are not particularly limited, and the material can be graphite, ceramic or metal (such as stainless steel).
[0117] Optionally, the annealing treatment includes the following steps: cooling from 700°C to 1000°C to room temperature, and the cooling time is ≥ 12 hours. Among them, 700°C to 1000°C is the starting temperature of the annealing treatment, and room temperature is the end temperature of the annealing treatment. The cooling rate of the annealing treatment can be calculated according to the requirements of the starting temperature, the end temperature and the cooling time.
[0118] Optionally, the cooling rate of the annealing treatment is 0.2℃ / min~1.5℃ / min, for example, 0.2℃ / min, 0.3℃ / min, 0.4℃ / min, 0.5℃ / min, 0.6℃ / min, 0.7℃ / min, 0.8℃ / min, 0.9℃ / min, 1℃ / min, 1.1℃ / min, 1.2℃ / min, 1.3℃ / min, 1.4℃ / min or 1.5℃ / min.
[0119] In some specific examples, the annealing treatment includes the following steps: pouring the molding material in the molding mold, transferring it to a high-temperature furnace or an annealing furnace, and slowly cooling it in the temperature range of 1000℃~700℃, with a cooling rate of 0.2℃ / min~1.5℃ / min, and a cooling time of ≥12h, until it cools to room temperature.
[0120] Optionally, after the annealing treatment, the method further includes the following steps: cutting, grinding, polishing and CNC (Computerized Numerical Control) processing the semi-finished glass after the annealing treatment.
[0121] Optionally, after the annealing treatment or after the CNC processing, the method further includes the following steps: placing the aluminosilicate glass in molten salt and chemically tempering it at 390° C. to 430° C. for 3 h to 8 h to prepare tempered aluminosilicate glass.
[0122] As an example, the molten salt may be one or more of LiNO3 molten salt, NaNO3 molten salt and KNO3 molten salt, and may further be NaNO3 molten salt and KNO3 molten salt, and may further be KNO3 molten salt and NaNO3 molten salt in a mass ratio of 96:4.
[0123] As an example, the temperature of the chemical tempering process may be 390°C, 395°C, 400°C, 405°C, 410°C, 415°C, 420°C, 425°C, or 430°C.
[0124] As an example, the chemical toughening treatment time may be 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 7.5 h or 8 h.
[0125] In a second aspect of the present application, an aluminosilicate glass is provided, which is prepared by the aluminosilicate glass preparation method as described above.
[0126] Optionally, the melting temperature (T m ) is 1580℃~1630℃. As an example, the melting temperature (T m ) can be 1580°C, 1585°C, 1590°C, 1595°C, 1600°C, 1605°C, 1610°C, 1615°C, 1620°C, 1625°C or 1630°C.
[0127] Optionally, the softening temperature (T s ) is 700℃~750℃. As an example, the softening temperature (T s ) can be 700°C, 705°C, 710°C, 715°C, 720°C, 725°C, 730°C, 735°C, 740°C, 745°C or 750°C.
[0128] Optionally, the linear expansion coefficient of aluminosilicate glass in the range of 30°C to 300°C is 90×10 -7 / ℃~100×10 -7As an example, the linear expansion coefficient of aluminosilicate glass in the range of 30°C to 300°C can be 90×10 -7 / ℃、91×10 -7 / ℃、92×10 -7 / ℃、93×10 -7 / ℃、94×10 -7 / ℃、95×10 -7 / ℃、96×10 -7 / ℃、97×10 -7 / ℃、98×10 -7 / ℃、99×10 -7 / ℃ or 100×10 -7 / ℃.
[0129] Optionally, the surface compressive stress (CS) of the aluminosilicate glass is 620 MPa to 900 MPa. As an example, the CS value of the aluminosilicate glass can be 620 MPa, 650 MPa, 680 MPa, 700 MPa, 720 MPa, 750 MPa, 780 MPa, 800 MPa, 820 MPa, 850 MPa, 880 MPa or 900 MPa.
[0130] Optionally, the stress layer depth (DOL) of the aluminosilicate glass is 28 μm to 45 μm. As an example, the DOL value of the aluminosilicate glass can be 28 μm, 29 μm, 30 μm, 31 μm, 32 μm, 33 μm, 34 μm, 35 μm, 36 μm, 37 μm, 38 μm, 39 μm, 40 μm, 41 μm, 42 μm, 43 μm, 44 μm or 45 μm.
[0131] In a third aspect of the present application, a cover glass is provided, which is made of the aluminosilicate glass as described above.
[0132] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.
[0133] Example 1
[0134] Please refer to Table 1. The aluminosilicate glass of this embodiment is composed of the following components in mass fractions: 58% SiO2, 13.5% Al2O3, 16.5% Na2O, 4.6% K2O, 3.9% MgO, 1.8% ZrO2, 1.2% B2O3 and 0.5% clarifier.
[0135] The method for preparing the aluminosilicate glass of this embodiment comprises the following steps:
[0136] (1) According to the above-mentioned formula of aluminosilicate glass, accurately weigh the required SiO2 source, Al2O3 source, Na2O source, K2O source, MgO source, ZrO2 source, B2O3 source, clarifier, binder and water.
[0137] The raw materials in the powder are as follows: SiO2 source is quartz sand, Al2O3 source is alumina, Na2O source is sodium carbonate, K2O source is potassium carbonate, MgO source is magnesium oxide, ZrO2 source is zirconium oxide, and B2O3 source is boric acid. The clarifier is composed of CeO2, SnO2 and NaNO3 in a mass ratio of 2:2:1. The binder is composed of Na2SiO3 and NaOH in a mass ratio of 2:1. The masses of the clarifier, binder, water and powder are a, b, c and d respectively, satisfying: a:b:c:(a+d)=0.5:3:1:100.
[0138] (2) Mix the clarifier, binder and water, and use a high-pressure spray gun atomization method to perform atomization treatment. The spray gun pressure is 0.3 MPa, the spray flow rate is 0.7 slm, and the atomization time is 8 min to obtain an atomized material; place the SiO2 source, Al2O3 source, Na2O source, K2O source, MgO source, ZrO2 source and B2O3 source in a mixer and mix for 10 min to obtain a powder; place the atomized material and the powder in a mixer and mix for 3 min to obtain a batch material.
[0139] (3) The batch is left to stand at room temperature for 12 hours to allow the binder to fully react with the remaining raw materials and precipitate crystalline compounds to obtain a crystalline material.
[0140] (4) The crystal material was placed in a circular tablet pressing mold (made of wear-resistant stainless steel, with a diameter of 10 mm and a thickness of 8 mm). A pressure of 6 tons was applied to the circular tablet pressing mold to obtain a bulk density of 2.138 g / cm 3 of bulk material.
[0141] (5) Place the block material in a platinum crucible, and place the platinum crucible in a kiln, heat it to 1580°C, and keep it at 1580°C for 6 hours to obtain molten glass; cool the molten glass to 1500°C~1550°C, and pour it into a graphite molding mold preheated to 500°C under normal temperature and pressure conditions; after the molten glass hardens, pour the molding material in the graphite molding mold, transfer it to a high-temperature furnace, and slowly cool it from 750°C at a cooling rate of 0.8°C / min for a cooling time of ≥12 hours until it cools to room temperature to obtain semi-finished glass.
[0142] (6) The semi-finished glass is taken out of the high-temperature furnace, cut, ground, polished and CNC processed, cleaned, and placed in a mixed molten salt (the mass ratio of KNO3 molten salt to NaNO3 molten salt is 96:4), and chemically tempered at 390°C for 7 hours to obtain tempered aluminosilicate glass.
[0143] Embodiments 2 to 16
[0144] The preparation methods of the aluminosilicate glasses of Examples 2 to 16 are basically the same as that of Example 1. The formulas and properties of each example are detailed in Tables 1 to 3.
[0145] Comparative Examples 1 to 6
[0146] The preparation methods of the aluminosilicate glasses of Comparative Examples 1 to 6 are basically the same as that of Example 1. The formulas and properties of the comparative examples are detailed in Table 4.
[0147] Comparative Example 7
[0148] The difference between Comparative Example 7 and Example 1 is that no atomization treatment is performed in step (2).
[0149] Step (2) is specifically as follows: SiO2 source, Al2O3 source, Na2O source, K2O source, MgO source, ZrO2 source, B2O3 source, clarifier, binder and water are mixed in a mixer for 12 minutes to obtain a batch material.
[0150] Comparative Example 8
[0151] The difference between Comparative Example 8 and Example 1 is that no crystallization reaction is performed, and the batch material is directly tableted.
[0152] Comparative Example 9
[0153] The difference between Comparative Example 9 and Example 1 is that no tableting process is performed, and the crystallized material is directly melted.
[0154] Comparative Example 10
[0155] This comparative example adopts a conventional preparation process. The specific preparation method of aluminosilicate glass is as follows: according to the formula of the aluminosilicate glass in Example 1, the required SiO2 source, Al2O3 source, Na2O source, K2O source, MgO source, ZrO2 source and B2O3 source are accurately weighed, and the materials are mixed in a mixer for 10 minutes to obtain a batch material; according to steps (5) to (6) of Example 1, the batch material is sequentially melted (melting temperature is 1598°C), formed, annealed, cut, ground, polished, CNC processed, cleaned and chemically toughened to obtain toughened aluminosilicate glass.
[0156] Test Case
[0157] The aluminosilicate glass was tested as follows, and the results are shown in Tables 1 to 5. The test objects of the linear expansion coefficient, softening temperature, melting temperature and number of bubbles in the range of 30°C to 300°C were the aluminosilicate glass after CNC processing and before chemical tempering, and the test objects of the CS value and DOL value were the aluminosilicate glass after chemical tempering.
[0158] (1) Bulk density of bulk material: It is determined based on the ratio of mass to volume of the bulk material, and the average bulk density of 10 bulk materials is taken.
[0159] (2) Coefficient of linear expansion (CTE): The coefficient of linear expansion of glass in the range of 30°C to 300°C was measured using a German NETZSCH DIL-402PC horizontal dilatometer with a heating rate of 5°C / min.
[0160] (3) Softening temperature (T s ): Measured according to standard ASTM C-338.
[0161] (4) Melting temperature (T m The viscosity was measured by using an Orton RSV-1600 high temperature viscometer from the United States, and the melting temperature was calculated according to the Vogel-Fulcher-Tamann formula.
[0162] (5) Stress properties: The CS value and DOL value of the glass were measured using the FSM-6000LE surface stress meter.
[0163] (6) Number of bubbles: Aluminosilicate glass was observed using a Leica polarizing microscope. The number of bubbles with a diameter of less than 0.1 mm was recorded and the number of bubbles per unit mass was calculated in pieces / kg.
[0164] According to Tables 1 to 3, the CTE (30°C to 300°C) of the aluminosilicate glasses of Examples 1 to 16 is 91.5×10 -7 / ℃~97.7×10 -7 / ℃,T s 708℃~745℃, T m The temperature of the aluminosilicate glass of Examples 1 to 16 is 1580° C. to 1630° C., the CS value after chemical tempering is 624 MPa to 855 MPa, and the DOL value is 29.0 μm to 41.8 μm. It can be seen that the aluminosilicate glasses of Examples 1 to 16 can obtain better physical and chemical properties.
[0165] According to Tables 4 and 5, the formula of Comparative Example 10 is the same as that of Example 1, but it is prepared by a conventional preparation process, resulting in the CTE (30°C~300°C) of the aluminosilicate glass increasing to 103.9×10-7 / ℃,T s Increased to 724℃, T m At the same time, the CS value and DOL value of the chemically tempered aluminosilicate glass are significantly lower than those in Example 1. It can be seen that compared with the traditional preparation process, the preparation processes of Examples 1 to 16 can effectively reduce the thermal properties such as melting temperature, softening temperature and thermal expansion coefficient, and can also improve the strengthening performance of aluminosilicate glass, which is conducive to obtaining tempered glass with high CS value and high DOL value.
[0166] With reference to Example 1, Comparative Example 7 did not undergo atomization treatment, and the binder, clarifier and water were not evenly dispersed in the batch material, resulting in a low bulk density of the block material produced in the subsequent tableting, which was easily broken into powder and scattered, and the unevenly dispersed clarifier failed to effectively promote the discharge of bubbles in the glass liquid, resulting in uniform glass components and many bubble defects; Comparative Example 8 did not undergo a crystallization reaction, resulting in difficulty in forming into a block material in the subsequent tableting process, or resulting in a low bulk density of the block material, which was easily broken into powder and scattered; Comparative Example 9 did not undergo a tableting reaction, and only relied on the crystallization reaction to form crystalline materials of different sizes, whose bulk density was low and difficult to measure, and which was easily broken into powder and scattered. It can be seen that the atomization treatment, crystallization reaction and tableting reaction in Example 1 are complementary and indispensable, and each step cooperates with each other to achieve the effects of inhibiting the scattering of raw materials, reducing the melting temperature, improving the strengthening effect, and increasing the yield of finished products.
[0167] The amount of the clarifier used in Comparative Example 1 is <0.1wt.%, and the amount of the clarifier used in Comparative Example 2 is >0.7wt.%, resulting in excessive bubbles in the aluminosilicate glass, and the CTE (30°C~300°C) cannot be measured. In addition, the aluminosilicate glass is prone to self-explosion during chemical tempering, making it difficult to measure the CS value and DOL value.
[0168] The amount of water used in Comparative Example 3 is too low, and the amount of binder used in Comparative Example 5 is too low, so the batch material cannot be formed into a block material through tableting, so the volume density of the block material cannot be measured. At the same time, during the melting process of Comparative Examples 3 and 5, some lightweight materials fly away, resulting in an increase in melting temperature and uneven composition of the finished glass, which in turn has an adverse effect on CTE, softening temperature and chemical tempering effect.
[0169] The amount of water used in Comparative Example 4 is too high, which causes the pressed block material to collapse easily or even fail to form. In addition, during the melting process, water bubbles in the glass liquid are difficult to discharge or require a longer clarification time, resulting in great difficulty in melting, which in turn has an adverse effect on CTE, softening temperature and chemical tempering effect.
[0170] The binder content in Comparative Example 6 is relatively high, resulting in a low bulk density of the block material. More fuel is required for melting during the melting process, which makes melting difficult, and thus has an adverse effect on CTE, softening temperature and chemical tempering effect.
[0171] In summary, the preparation methods of aluminosilicate glass provided in Examples 1 to 16 can effectively improve the uniformity of mixing and the melting rate, reduce the melting temperature, and reduce the scattering of raw materials, and have the advantages of stable glass composition, good physical and chemical properties, high yield of finished products, and low cost, which is conducive to industrial mass production. At the same time, the formulas provided in Examples 1 to 16 are more conducive to obtaining aluminosilicate glass with better intrinsic mechanical properties and chemical tempering effects.
[0172] Table 1. Formulations and properties of aluminosilicate glasses of Examples 1 to 6
[0173]
[0174] Table 2. Formulations and properties of aluminosilicate glasses of Examples 7 to 12
[0175]
[0176] Table 3. Formulations and properties of aluminosilicate glasses of Examples 13 to 16
[0177]
[0178] Table 4. Formulas and properties of aluminosilicate glasses of comparative examples 1 to 6
[0179]
[0180] Note: “--” in Table 4 means that the parameter cannot be measured.
[0181] Table 5. Formulas and properties of aluminosilicate glasses of comparative examples 7 to 10
[0182]
[0183] Note: “--” in Table 5 means that the parameter cannot be measured.
[0184] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0185] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of protection of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the scope of protection of the present application. Therefore, the scope of protection of the present application shall be subject to the attached claims.
Claims
1. A method for preparing aluminosilicate glass, characterized in that: The following steps are involved: Mixing a clarifier, a binder and water, performing atomization treatment to prepare an atomized material, and mixing the remaining raw materials of the aluminosilicate glass to prepare a powder material; Mixing the atomized material and the powder material to prepare a batch material; Allowing the batch material to undergo a crystallization reaction to prepare a crystallized material; The crystallized material is tableted to prepare a block material; Performing melting treatment, molding treatment and annealing treatment on the block material to prepare the aluminosilicate glass; Wherein, the binder includes one or more of sodium silicate, sodium hydroxide and sodium carbonate; The masses of the clarifier, the binder, the water and the powder are a, b, c and d respectively, satisfying: a:b:c:(a+d)=(0.1~0.7):(2~9):(1~8):
100.
2. The method for preparing aluminosilicate glass according to claim 1, characterized in that: The aluminosilicate glass comprises the following components by mass fraction: 。 3. The method for preparing aluminosilicate glass according to claim 2, characterized in that: The clarifier includes one or more of tin oxide, antimony oxide, cerium oxide, sodium sulfate, barium sulfate, calcium sulfate, sodium nitrate, ammonium nitrate, sodium chloride, ammonium chloride, calcium fluoride and sodium fluorosilicate.
4. The method for preparing aluminosilicate glass according to any one of claims 1 to 3, characterized in that: The atomization treatment methods independently include one or more of high-pressure spray gun atomization, ultrasonic atomization and rotary atomization.
5. The method for preparing aluminosilicate glass according to claim 4, characterized in that: One or more of the following conditions are met: (1) The spray gun pressure of the high-pressure spray gun atomization method is 0.3MPa~0.8MPa; (2) The spray flow rate of the high-pressure spray gun atomization method is 0.5slm~2slm; (3) The atomization time of the atomization treatment is 10 min to 20 min.
6. The method for preparing aluminosilicate glass according to any one of claims 1 to 3, characterized in that: The batch material is subjected to a crystallization reaction, comprising the following steps: The batch material is allowed to stand at room temperature for 4 h to 24 h.
7. The method for preparing aluminosilicate glass according to any one of claims 1 to 3, characterized in that: The crystallized material is tabletted, comprising the following steps: The crystal material is placed in a tableting mold and a pressure of 2t to 8t is applied to make the bulk density of the block material ≥1.9g / cm 3 .
8. The method for preparing aluminosilicate glass according to any one of claims 1 to 3, characterized in that: One or more of the following conditions are met: (1) The melting treatment comprises the following steps: keeping the temperature at 1580°C to 1630°C for 4h to 8h; (2) The molding method includes a casting molding method; (3) The annealing treatment comprises the following steps: cooling from 700°C to 1000°C to room temperature, and the cooling time is ≥ 12h.
9. The method for preparing aluminosilicate glass according to any one of claims 1 to 3, characterized in that: After the annealing treatment, the following steps are also included: The aluminosilicate glass is placed in molten salt and chemically toughened at 390° C. to 430° C. for 3 h to 8 h.
10. An aluminosilicate glass, characterized in that: The aluminosilicate glass is prepared by the method for preparing the aluminosilicate glass according to any one of claims 1 to 9.
11. The aluminosilicate glass according to claim 10, characterized in that One or more of the following conditions are met: (1) The melting temperature of the aluminosilicate glass is 1580°C to 1630°C; (2) The softening temperature of the aluminosilicate glass is 700°C to 750°C; (3) The linear expansion coefficient of the aluminosilicate glass in the range of 30°C to 300°C is 90×10 -7 / ℃~100×10 -7 / ℃; (4) The surface compressive stress of the aluminosilicate glass is 620 MPa to 900 MPa; (5) The stress layer depth of the aluminosilicate glass is 28 μm to 45 μm.
12. A cover glass, characterized in that: It is made of the aluminosilicate glass as claimed in claim 10 or 11.
Citation Information
Cited By
Composite clarifying agent for photovoltaic glass as well as preparation method and application of composite clarifying agent
CN119874181A