Modified polytetrafluoroethylene as well as preparation method and application thereof

By introducing polyetheretherketone, modified fillers and silane coupling agents into polytetrafluoroethylene, combined with ammonia plasma modification and polypropylene alcohol grafting technology, the problem of insufficient performance of polytetrafluoroethylene at extreme temperatures is solved. problem, significantly improving its mechanical strength, compressive resistance and tribological properties, making it suitable for a wider range of working environments.

CN118852883APending Publication Date: 2024-10-29CIXI HIGH NEW COXIN SEALING MATERIAL
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410945153.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing PTFE sealing products show shortcomings such as low cold flow resistance, poor creep resistance, high hardness, and poor resilience under extreme temperature environments. Moreover, their surface activity is extremely low, making it difficult to be compatible with fillers and causing uneven dispersion. The filler reinforcement effect is uneven and affects the mechanical properties.

Method used

It uses components such as polytetrafluoroethylene, polyetheretherketone, modified fillers, calcium stearate and silane coupling agent, and improves the mechanical strength of the material through ammonia plasma modification and polypropylene alcohol grafting. Compressive properties, creep deformation properties and tribological properties, and through the synergistic effect of modified fillers and silane coupling agents, the material structure and compatibility are optimized.

Benefits of technology

It has achieved the excellent performance of polytetrafluoroethylene in the range of -235°C to +300°C, including improvements in mechanical strength, compressive resistance, creep deformation performance and tribological properties, to meet the needs of long-term effective work.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004945413640000071
    Figure BDA0004945413640000071
  • Figure BDA0004945413640000081
    Figure BDA0004945413640000081
Patent Text Reader

Abstract

The invention relates to the technical field of polytetrafluoroethylene preparation, in particular to modified polytetrafluoroethylene as well as a preparation method and application thereof. The modified polytetrafluoroethylene is prepared from the following raw materials in parts by mass: 50 to 55 parts of polytetrafluoroethylene, 8 to 12 parts of polyether-ether-ketone, 10 to 12 parts of modified filler, 0.2 to 0.3 part of calcium stearate and 2 to 3 parts of silane coupling agent. The prepared modified polytetrafluoroethylene has excellent performance in engineering application, the reliability and durability of the sealing material can be effectively improved, and various requirements in high-temperature and low-temperature environments are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polytetrafluoroethylene preparation, and in particular to a modified polytetrafluoroethylene and a preparation method and application thereof. Background Art

[0002] Gaskets are mechanical seals between two objects, usually used to prevent leakage due to pressure, corrosion, and natural thermal expansion and contraction of pipelines. Since the machined surface cannot be perfect, gaskets can be used to fill irregularities. Gaskets are usually made of sheet materials, such as pad paper, rubber, silicone rubber, metal, cork, felt, neoprene, nitrile rubber, fiberglass or plastic polymers.

[0003] Polytetrafluoroethylene has high chemical stability, excellent high and low temperature resistance, outstanding non-stickiness, good lubricity and wear resistance, and is the preferred material for gaskets; however, the price of polytetrafluoroethylene is relatively high, and its rigidity is relatively large, its shock absorption and buffering effect is average, and it is not easy to form a stable sealing polytetrafluoroethylene product.

[0004] Because of its super corrosion resistance, chemical stability, good dielectric properties, anti-aging, mechanical tensile strength, non-stickiness, low friction coefficient and good weather resistance, it is widely used in the fields of chemistry, industry, medicine, etc. However, it is inevitable that the surface activity of polytetrafluoroethylene is extremely low, it is difficult to be compatible with fillers, the unevenly dispersed fillers have uneven reinforcement effects, the overall creep improvement is poor, and the mechanical properties of the polytetrafluoroethylene body are affected relatively little. At present, ordinary polytetrafluoroethylene sealing products have the following defects: low cold flow resistance, poor creep resistance, high hardness, poor resilience, etc. Market application practice has shown that ordinary polytetrafluoroethylene gaskets can still meet the use conditions in the range of -55℃—180℃, and the tribological properties are significantly weakened beyond this temperature range. Summary of the invention

[0005] The purpose of this application is to provide a modified polytetrafluoroethylene and its preparation method and application in view of the deficiencies of the current technology. The modified polytetrafluoroethylene prepared in this application has excellent mechanical strength, compressive resistance, creep deformation performance and tribological properties, and can work effectively for a long time in a working environment of -235°C to +300°C.

[0006] In the first aspect, the present application provides a modified polytetrafluoroethylene, which adopts the following technical solution: A modified polytetrafluoroethylene comprises the following raw materials by weight: 50-55 parts of polytetrafluoroethylene, 8-12 parts of polyetheretherketone, 10-12 parts of modified filler, 0.2-0.3 parts of calcium stearate and 2-3 parts of silane coupling agent.

[0007] By adopting the above technical solutions, polytetrafluoroethylene: as a basic raw material, it has excellent high temperature resistance and chemical inertness, and is the main component of modified polytetrafluoroethylene. Polyetheretherketone: improves the wear resistance of modified polytetrafluoroethylene, enhances its mechanical strength, and also has good stability at elevated working temperatures. Modified filler: through the introduction of modified fillers, the problem of poor affinity of polytetrafluoroethylene is compensated, the compatibility and dispersibility of modified polytetrafluoroethylene and fillers are improved, and the mechanical strength, compressive resistance, creep deformation performance and tribological properties are improved. Calcium stearate: as a stabilizer, it can enhance the thermal stability of modified polytetrafluoroethylene and extend its service life in high temperature environments. Silane coupling agent: through the coupling effect, the modified filler and polytetrafluoroethylene are effectively combined together, which improves the dispersibility of the filler and the performance of the modified polytetrafluoroethylene. Through the effects and synergistic effects of the above components, the modified polytetrafluoroethylene has excellent performance in the working environment, including mechanical strength, high temperature resistance, wear resistance, creep deformation performance and tribological properties are improved, meeting the needs of long-term effective work in the working environment of -235℃ to +300℃.

[0008] Preferably, the polytetrafluoroethylene is polypropylene alcohol grafted polytetrafluoroethylene, and the modification method of the polypropylene alcohol grafted polytetrafluoroethylene comprises the following steps: S21, vacuum drying the polytetrafluoroethylene particles and placing them in a plasma treatment device for ammonia plasma modification, wherein the discharge voltage of the ammonia plasma modification is 4 kV, the time is 40-50 s, the working gas flow rate is 7 L / min, the working gas is a mixed gas of ammonia and helium, and the volume ratio of ammonia to helium is 1:50, to obtain amino-modified polytetrafluoroethylene; S22, subjecting the amino-modified polytetrafluoroethylene to plasma treatment, wherein the plasma is polypropylene alcohol vapor, the treatment power is 200 W, and the treatment time is 8-10 minutes, to obtain polypropylene alcohol grafted polytetrafluoroethylene.

[0009] By adopting the above technical scheme, the polytetrafluoroethylene particles are modified by ammonia plasma to make their surface amino, thereby improving their wettability. This modification can greatly improve the reactivity of the polytetrafluoroethylene surface, providing conditions for the subsequent polypropylene alcohol grafting. The amino polytetrafluoroethylene is further treated with plasma, using polypropylene alcohol vapor as a plasma source to obtain polypropylene alcohol grafted polytetrafluoroethylene. This step increases the reaction sites on the polytetrafluoroethylene, enhances the compatibility with the modified filler, and improves the uniformity of the material properties and the degree of polymerization between the molecular chains, thereby improving the mechanical strength, compressive resistance, creep deformation performance and tribological properties of the modified polytetrafluoroethylene.

[0010] Preferably, the method for preparing the modified filler comprises the following steps: S31, diluting 2,2,2-trifluoroethylamine with acetone, introducing nitrogen protection, controlling the temperature of a water bath to 40-45°C, stirring and adding triethylamine to mix, then slowly adding γ-aminopropyltriethoxysilane, controlling the reaction time of adding γ-aminopropyltriethoxysilane to 2-2.5h, and removing acetone by rotary evaporation after the reaction to obtain modified γ-aminopropyltriethoxysilane; S32. Mix the modified γ-aminopropyltriethoxysilane, ethanol and deionized water, adjust the pH value of the mixture to 5.2 with hydrochloric acid, add the filler and stir to mix, heat to 35°C, let stand for coupling for 12 hours, and after the reaction is completed, filter, wash and dry to obtain the modified filler.

[0011] By adopting the above technical scheme, γ-aminopropyltriethoxysilane and 2,2,2-trifluoroethylamine are opened to prepare modified γ-aminopropyltriethoxysilane with a fluorine-containing structure, and then graphene nanosheets, barium sulfate and nano-titanium dioxide are used as fillers. The modified γ-aminopropyltriethoxysilane is attached to the surface of the filler through chelation to form a chelation-coupling loading mechanism, which compensates for the poor affinity of fluoride, improves the compatibility and dispersibility of the modified filler with polytetrafluoroethylene, and thus improves the mechanical strength, compressive resistance, creep deformation performance and tribological properties of the modified polytetrafluoroethylene.

[0012] Preferably, in step S31, the usage ratio of γ-aminopropyltriethoxysilane, 2,2,2-trifluoroethylamine, triethylamine and acetone is 1 mol: 1 mol: 55 mL: 600-700 mL.

[0013] Preferably, in step S32, the usage ratio of the filler, modified γ-aminopropyltriethoxysilane, ethanol and deionized water is 100 g:15 g:100 mL:30 mL.

[0014] Preferably, the filler is prepared by mixing graphene nanosheets, barium sulfate and nano-titanium dioxide in a mass ratio of 1:30:12, the graphene nanosheets have a sheet thickness of 20 nm and a sheet diameter of 10-20 μm, the barium sulfate has a particle size of 20 μm, and the nano-titanium dioxide has a particle size of 80 nm.

[0015] By adopting the above technical solution, the graphene nanosheets, barium sulfate and nano-titanium dioxide used have special sizes and characteristics. The synergistic effect between them helps to optimize the structure of polytetrafluoroethylene at the micro level and further improve the mechanical strength, compressive resistance, creep deformation performance and tribological properties of modified polytetrafluoroethylene.

[0016] Preferably, the silane coupling agent is prepared by mixing hexadecyltrimethoxysilane and γ-aminopropyltriethoxysilane in a mass ratio of 2:8.

[0017] By adopting the above technical scheme, silane coupling agent plays an important role in the preparation of modified polytetrafluoroethylene. The silane coupling agent prepared by mixing hexadecyltrimethoxysilane and γ-aminopropyltriethoxysilane in a mass ratio of 2:8 can improve the compatibility of the modified filler and polytetrafluoroethylene and promote the bonding between the two. The silane coupling agent can improve the interaction force between the surface of the modified filler and polytetrafluoroethylene, thereby enhancing the adhesion and compatibility between the two. This helps the modified filler to be evenly dispersed in the polytetrafluoroethylene matrix and improve the performance stability and mechanical strength of the modified polytetrafluoroethylene. The hexadecyltrimethoxysilane and γ-aminopropyltriethoxysilane in the silane coupling agent have different functional groups, which can react chemically with the filler surface and the polytetrafluoroethylene matrix at the same time to form an organic / inorganic hybrid structure, thereby enhancing the bonding strength between the two. The role of hexadecyltrimethoxysilane in silane coupling agent is similar to that of hydrophobic agent. It can form a protective film on the surface of polytetrafluoroethylene matrix, improve its wettability and wear resistance, and reduce surface energy at the same time, which helps to reduce surface tension and improve the interface interaction between filler and matrix. Silane coupling agent can improve the performance of modified polytetrafluoroethylene by improving the dispersibility of filler, increasing its contact area with polytetrafluoroethylene, promoting the cross-linking reaction between filler and matrix. In the preparation of modified polytetrafluoroethylene, the addition of silane coupling agent can cooperate with modified filler and other raw materials such as polyetheretherketone to comprehensively improve the performance of modified polytetrafluoroethylene, including mechanical strength, compressive resistance, creep deformation performance and tribological properties.

[0018] In a second aspect, the present application provides a method for preparing modified polytetrafluoroethylene, which adopts the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned modified polytetrafluoroethylene, comprising the following steps: S81, according to the mass fractions, polytetrafluoroethylene, polyetheretherketone, modified filler, calcium stearate and silane coupling agent are put into a planetary mixer, and stirred and mixed evenly to obtain a mixed raw material; S82, filling the mixed raw materials into the mold and scraping it flat, maintaining the pressure at 80 MPa for 1-2 minutes, cold pressing and shaping, and making a blank; S83, sending the blank into a sintering furnace, performing hot sintering, and obtaining modified polytetrafluoroethylene after cooling.

[0019] Preferably, the process conditions of the thermal sintering are: the heating rate is controlled at 10°C / min within 290°C, and the heating rate is controlled at 1°C / min at 290-380°C; the temperature is kept at 380°C for 160-180min; during the cooling process, the temperature is within the range of 280-380°C, the cooling rate is controlled at 2°C / min, and the temperature is kept at 300-320°C for 30-50min, and the rate in the remaining temperature sections is controlled at 5°C / min.

[0020] In a third aspect, the present application provides an application of modified polytetrafluoroethylene, using the following technical solution: As a general technical concept, the present application also provides the use of the above-mentioned modified polytetrafluoroethylene in sealing products.

[0021] In summary, the beneficial technical effects of this application are: 1. Excellent mechanical strength: By adding polyetheretherketone and modified fillers, as well as ammonia plasma modification and grafting of polytetrafluoroethylene particles, the mechanical strength of modified polytetrafluoroethylene is improved, so that it can still maintain stable performance in high and extremely low temperature environments.

[0022] 2. Excellent compressive performance: Modified fillers and amination treatment help to enhance the wettability of the PTFE surface, improve the compressive performance of modified PTFE, and make it perform better in sealing applications.

[0023] 3. Excellent creep deformation performance: Through the chelation of modified fillers and the increase of internal polymerization degree, the creep deformation performance of modified polytetrafluoroethylene is improved, so that it can maintain stable performance under long-term working conditions.

[0024] 4. Excellent tribological properties: The addition of raw materials such as calcium stearate and silane coupling agent, combined with the characteristics of modified fillers, improves the tribological properties of modified polytetrafluoroethylene, making it suitable for a wider range of working environments.

[0025] 5. Excellent temperature resistance: The modified polytetrafluoroethylene can maintain stable performance under extreme temperature conditions (-235℃ to +300℃), thanks to the inherent characteristics of polytetrafluoroethylene and the optimization of material structure and surface properties during the modification process. DETAILED DESCRIPTION

[0026] The embodiments of the present application will be described in detail below in conjunction with the examples, but those skilled in the art will understand that the following examples are only used to illustrate the present application and should not be considered to limit the scope of the present application. If no specific conditions are specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer.

[0027] Preparation Example 1 Polypropylene alcohol grafted polytetrafluoroethylene The modification method of polypropylene alcohol grafted polytetrafluoroethylene comprises the following steps: S21, vacuum drying the polytetrafluoroethylene particles and placing them in a plasma treatment device for ammonia plasma modification, wherein the discharge voltage of the ammonia plasma modification is 4 kV, the time is 45 s, the working gas flow rate is 7 L / min, the working gas is a mixed gas of ammonia and helium, and the volume ratio of ammonia to helium is 1:50, to obtain amino-modified polytetrafluoroethylene; S22, subjecting the amino-modified polytetrafluoroethylene to plasma treatment, wherein the plasma is polypropylene alcohol vapor, the treatment power is 200 W, and the treatment time is 9 minutes, to obtain polypropylene alcohol grafted polytetrafluoroethylene.

[0028] The polypropylene alcohol grafted polytetrafluoroethylene prepared above is used as the polytetrafluoroethylene raw material in various embodiments.

[0029] Preparation Example 2 Preparation of modified filler The preparation method of the modified filler comprises the following steps: S31, dilute 1 mol of 2,2,2-trifluoroethylamine with 650 mL of acetone, introduce nitrogen protection, control the temperature of the water bath to 43°C, stir and add 1 mol of triethylamine to mix, then slowly add 1 mol of γ-aminopropyltriethoxysilane, control the addition reaction time of γ-aminopropyltriethoxysilane to 2.3 h, and remove acetone by rotary evaporation after the reaction to obtain modified γ-aminopropyltriethoxysilane; S32. Mix 150g of modified γ-aminopropyltriethoxysilane, 1000mL of ethanol and 300mL of deionized water, adjust the pH value of the mixture to 5.2 with hydrochloric acid, add 1000g of filler and stir to mix, heat to 35°C, let stand for coupling for 12h, and after the reaction is completed, filter, wash and dry to obtain a modified filler, wherein the filler is prepared by mixing graphene nanosheets, barium sulfate and nano-titanium dioxide in a mass ratio of 1:30:12, the graphene nanosheets have a sheet thickness of 20nm, a sheet diameter of 10-20μm, the barium sulfate particle size is 20μm, and the nano-titanium dioxide particle size is 80nm.

[0030] The modified filler prepared above was applied to various examples.

[0031] Preparation Comparative Example 1 The method is the same as Preparation Example 2, except that the filler is a graphene nanosheet, the graphene nanosheet has a sheet thickness of 20 nm, and a sheet diameter of 10-20 μm.

[0032] Preparation Comparative Example 2 The same as Preparation Example 2, except that: the filler is barium sulfate, and the particle size of the barium sulfate is 20 μm.

[0033] Preparation Comparative Example 3 The same as Preparation Example 2, except that: the filler is nano titanium dioxide, and the particle size of the nano titanium dioxide is 80 nm.

[0034] Example 1 A modified polytetrafluoroethylene comprises the following raw materials, measured by weight: 5.0 kg of polytetrafluoroethylene, 0.8 kg of polyetheretherketone, 1.0 kg of modified filler, 0.02 kg of calcium stearate, and 0.2 kg of a silane coupling agent, wherein the silane coupling agent is prepared by mixing hexadecyltrimethoxysilane and gamma-aminopropyltriethoxysilane in a weight ratio of 2:8.

[0035] The above-mentioned method for preparing modified polytetrafluoroethylene comprises the following steps: S81. Put polytetrafluoroethylene, polyetheretherketone, modified filler, calcium stearate and silane coupling agent into a planetary mixer according to their weight proportions, and stir and mix them evenly to obtain a mixed raw material; S82, filling the mixed raw materials into the mold and scraping it flat, maintaining the pressure at 80 MPa for 1 minute, cold pressing and shaping, and forming a blank; S83. The blank is sent into a sintering furnace for hot sintering. The process conditions of the hot sintering are: the heating rate is controlled at 10°C / min within 290°C, and the heating rate is controlled at 1°C / min in the range of 290-380°C; the temperature is kept at 380°C for 160 minutes; during the cooling process, the temperature is within the range of 280-380°C, the cooling rate is controlled at 2°C / min, and the temperature is kept at 300°C for 50 minutes. The rate in the remaining temperature sections is controlled at 5°C / min. After cooling, modified polytetrafluoroethylene is obtained.

[0036] Example 2 A modified polytetrafluoroethylene comprises the following raw materials, measured by weight: 5.5 kg of polytetrafluoroethylene, 1.2 kg of polyetheretherketone, 1.2 kg of modified filler, 0.03 kg of calcium stearate, and 0.3 kg of a silane coupling agent, wherein the silane coupling agent is prepared by mixing hexadecyltrimethoxysilane and gamma-aminopropyltriethoxysilane in a weight ratio of 2:8.

[0037] The above-mentioned method for preparing modified polytetrafluoroethylene comprises the following steps: S81. Put polytetrafluoroethylene, polyetheretherketone, modified filler, calcium stearate and silane coupling agent into a planetary mixer according to their weight proportions, and stir and mix them evenly to obtain a mixed raw material; S82, filling the mixed raw materials into the mold and scraping it flat, maintaining the pressure at 80 MPa for 2 minutes, cold pressing and shaping, and forming a blank; S83. The blank is sent into a sintering furnace for hot sintering. The process conditions of the hot sintering are: the heating rate is controlled at 10°C / min within 290°C, and the heating rate is controlled at 1°C / min in the range of 290-380°C; the temperature is kept at 380°C for 180 minutes; during the cooling process, the temperature is within the range of 280-380°C, the cooling rate is controlled at 2°C / min, and the temperature is kept at 320°C for 30 minutes. The rates in the remaining temperature sections are controlled at 5°C / min. After cooling, modified polytetrafluoroethylene is obtained.

[0038] Example 3 A modified polytetrafluoroethylene comprises the following raw materials, measured by weight: 5.3 kg of polytetrafluoroethylene, 1 kg of polyetheretherketone, 1.1 kg of modified filler, 0.025 kg of calcium stearate, and 0.25 kg of a silane coupling agent, wherein the silane coupling agent is prepared by mixing hexadecyltrimethoxysilane and gamma-aminopropyltriethoxysilane in a weight ratio of 2:8.

[0039] The above-mentioned method for preparing modified polytetrafluoroethylene comprises the following steps: S81. Put polytetrafluoroethylene, polyetheretherketone, modified filler, calcium stearate and silane coupling agent into a planetary mixer according to their weight proportions, and stir and mix them evenly to obtain a mixed raw material; S82, fill the mixed raw materials into the mold and scrape it flat, maintain the pressure at 80MPa for 1.5min, cold press to shape, and make a blank; S83, send the blank into a sintering furnace for hot sintering, and the process conditions of the hot sintering are: the heating rate is controlled at 10℃ / min within 290℃, and the heating rate is controlled at 1℃ / min at 290-380℃; keep warm at 380℃ for 170min; during the cooling process, keep in the temperature range of 280-380℃, control the cooling rate at 2℃ / min, keep warm at 310℃ for 40min, and control the rate in the remaining temperature sections at 5℃ / min. After cooling, modified polytetrafluoroethylene is obtained.

[0040] Comparative Example 1 The same as Example 3, except that the modified filler is the modified filler prepared in Comparative Example 1.

[0041] Comparative Example 2 The same as Example 3, except that the modified filler is the modified filler prepared in Comparative Example 2.

[0042] Comparative Example 3 The same as Example 3, except that the modified filler is the modified filler prepared in Comparative Example 3.

[0043] Comparative Example 4 The same as Example 3, except that an equal amount of filler (the filler is prepared by mixing graphene nanosheets, barium sulfate and nano-titanium dioxide in a mass ratio of 1:30:12, the graphene nanosheets have a sheet thickness of 20 nm, a sheet diameter of 10-20 μm, the barium sulfate particle size is 20 μm, and the nano-titanium dioxide particle size is 80 nm) is used instead of the modified filler.

[0044] Comparative Example 5 The same as Example 3, except that the coupling agent is hexadecyltrimethoxysilane.

[0045] Comparative Example 6 The same as Example 3, except that the coupling agent is γ-aminopropyltriethoxysilane.

[0046] Comparative Example 7 The same as Example 3, except that the polytetrafluoroethylene is polytetrafluoroethylene that has not been modified by the preparation method of the present application.

[0047] Performance Testing The modified polytetrafluoroethylene prepared in Examples 1 to 3 and Comparative Examples 1 to 7 was sampled and subjected to the following performance tests. The test results are shown in Table 1. The tensile performance test and bending performance test are carried out using INSTRONG universal testing machine. The tensile test standard complies with the national standard GB / T1040.1-2006, and the bending test complies with the national standard GB / T 9341-2008. Compression performance: Compression performance test was carried out according to GB / T 1041-2008 standard, with a compression rate of 5 mm / min; Creep performance: creep performance test was carried out according to ASTMD621-1988 standard, the test pressure was 10MPa, the test time was 48h, and the test temperature was 25℃; Friction coefficient and wear scar width: tested in accordance with GB / T 3960, with a test load of 200N and a linear speed of 0.43m / s (diameter of the metal pair ring is 40nm and the rotation speed is 200rpm). Table 1 Performance test Analyzing the data in Table 1, we can see that: 1) The modified polytetrafluoroethylene prepared in Examples 1 to 3 has excellent mechanical strength, compressive resistance, creep deformation performance and tribological properties, and can work effectively for a long time in a working environment of -235°C to +300°C.

[0048] 2) The performance comparison analysis of the modified polytetrafluoroethylene prepared in combination with Example 3 and Comparative Examples 1 to Comparative Examples 4 shows that the modified γ-aminopropyltriethoxysilane with a fluorine-containing structure is prepared by ring-opening γ-aminopropyltriethoxysilane and 2,2,2-trifluoroethylamine, and then graphene nanosheets, barium sulfate and nano-titanium dioxide are used as fillers. The modified γ-aminopropyltriethoxysilane is attached to the surface of the filler through chelation to form a chelation-coupling loading mechanism, which compensates for the poor affinity of fluoride, improves the compatibility and dispersibility of the modified filler with polytetrafluoroethylene, and thus improves the mechanical strength, compressive resistance, creep deformation performance and tribological properties of the modified polytetrafluoroethylene; the graphene nanosheets, barium sulfate and nano-titanium dioxide used have special sizes and characteristics, and the synergistic effect between them helps to optimize the structure of polytetrafluoroethylene at the microscopic level, and further improves the mechanical strength, compressive resistance, creep deformation performance and tribological properties of the modified polytetrafluoroethylene.

[0049] 3) The performance comparison analysis of the modified polytetrafluoroethylene obtained in combination with Example 3 and Comparative Examples 5-6 shows that the silane coupling agent is prepared by mixing hexadecyl trimethoxysilane and γ-aminopropyl triethoxysilane in a mass fraction ratio of 2:8, which can improve the interaction force between the surface of the modified filler and the polytetrafluoroethylene, thereby enhancing the adhesion and compatibility between the two. This helps the modified filler to be uniformly dispersed in the polytetrafluoroethylene matrix, thereby improving the performance stability and mechanical strength of the modified polytetrafluoroethylene. The hexadecyl trimethoxysilane and γ-aminopropyl triethoxysilane in the silane coupling agent have different functional groups, which can react chemically with the filler surface and the polytetrafluoroethylene matrix at the same time to form an organic / inorganic hybrid structure, thereby enhancing the bonding strength between the two. The performance of the modified polytetrafluoroethylene can be improved by improving the dispersibility of the filler, increasing its contact area with polytetrafluoroethylene, promoting the cross-linking reaction between the filler and the matrix. By utilizing the synergistic effect between them, modified fillers and other raw materials such as polyetheretherketone, the properties of modified polytetrafluoroethylene, including mechanical strength, compressive resistance, creep deformation performance and tribological properties, are comprehensively improved.

[0050] 4) The performance comparison analysis of the modified polytetrafluoroethylene obtained in combination with Example 3 and Comparative Example 7 shows that the polytetrafluoroethylene particles are modified by ammonia plasma to make their surfaces aminized, thereby improving their wettability. This modification can greatly improve the reactivity of the polytetrafluoroethylene surface, providing conditions for the subsequent polypropylene alcohol grafting. The aminized polytetrafluoroethylene is further subjected to plasma treatment, using polypropylene alcohol vapor as a plasma source to obtain polypropylene alcohol grafted polytetrafluoroethylene. This step increases the reaction sites on the polytetrafluoroethylene, enhances the compatibility with the modified filler, and improves the uniformity of the material properties and the degree of polymerization between the molecular chains, thereby further improving the mechanical strength, compressive properties, creep deformation properties and tribological properties of the modified polytetrafluoroethylene.

[0051] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.

Claims

1. A modified polytetrafluoroethylene, characterized in that: The preparation raw materials include the following by weight: 50-55 parts of polytetrafluoroethylene, 8-12 parts of polyetheretherketone, 10-12 parts of modified filler, 0.2-0.3 parts of calcium stearate and 2-3 parts of silane coupling agent.

2. A modified polytetrafluoroethylene according to claim 1, characterized in that: The polytetrafluoroethylene is polypropylene alcohol grafted polytetrafluoroethylene, and the modification method of the polypropylene alcohol grafted polytetrafluoroethylene comprises the following steps: S21, vacuum drying the polytetrafluoroethylene particles and placing them in a plasma treatment device for ammonia plasma modification, wherein the discharge voltage of the ammonia plasma modification is 4 kV, the time is 40-50 s, the working gas flow rate is 7 L / min, the working gas is a mixed gas of ammonia and helium, and the volume ratio of ammonia to helium is 1:50, to obtain amino-modified polytetrafluoroethylene; S22, subjecting the amino-modified polytetrafluoroethylene to plasma treatment, wherein the plasma is polypropylene alcohol vapor, the treatment power is 200 W, and the treatment time is 8-10 minutes, to obtain polypropylene alcohol grafted polytetrafluoroethylene.

3. The modified polytetrafluoroethylene according to claim 1, characterized in that: The preparation method of the modified filler comprises the following steps: S31, diluting 2,2,2-trifluoroethylamine with acetone, introducing nitrogen protection, controlling the temperature of a water bath to 40-45°C, stirring and adding triethylamine to mix, then slowly adding γ-aminopropyltriethoxysilane, controlling the reaction time of adding γ-aminopropyltriethoxysilane to 2-2.5h, and removing acetone by rotary evaporation after the reaction to obtain modified γ-aminopropyltriethoxysilane; S32. Mix the modified γ-aminopropyltriethoxysilane, ethanol and deionized water, adjust the pH value of the mixture to 5.2 with hydrochloric acid, add the filler and stir to mix, heat to 35°C, let stand for coupling for 12 hours, and after the reaction is completed, filter, wash and dry to obtain the modified filler.

4. A modified polytetrafluoroethylene according to claim 3, characterized in that: In step S31, the usage ratio of γ-aminopropyltriethoxysilane, 2,2,2-trifluoroethylamine, triethylamine and acetone is 1 mol: 1 mol: 55 mL: 600-700 mL.

5. A modified polytetrafluoroethylene according to claim 3, characterized in that: In step S32, the usage ratio of the filler, modified γ-aminopropyltriethoxysilane, ethanol and deionized water is 100 g:15 g:100 mL:30 mL.

6. The modified polytetrafluoroethylene according to claim 3, characterized in that: The filler is prepared by mixing graphene nanosheets, barium sulfate and nano-titanium dioxide in a mass ratio of 1:30:

12. The graphene nanosheets have a sheet thickness of 20nm and a sheet diameter of 10-20μm. The barium sulfate has a particle size of 20μm and the nano-titanium dioxide has a particle size of 80nm.

7. The modified polytetrafluoroethylene according to claim 1, characterized in that: The silane coupling agent is prepared by mixing hexadecyltrimethoxysilane and gamma-aminopropyltriethoxysilane in a mass ratio of 2:

8.

8. A method for preparing modified polytetrafluoroethylene as claimed in any one of claims 1 to 7, characterized in that: The following steps are involved: S81. Put polytetrafluoroethylene, polyetheretherketone, modified filler, calcium stearate and silane coupling agent into a planetary mixer according to their weight proportions, and stir and mix them evenly to obtain a mixed raw material; S82, filling the mixed raw materials into the mold and scraping it flat, maintaining the pressure at 80 MPa for 1-2 minutes, cold pressing and shaping, and forming a blank; S83, sending the blank into a sintering furnace for thermal sintering, and obtaining modified polytetrafluoroethylene after cooling.

9. The method for preparing modified polytetrafluoroethylene according to claim 8, characterized in that: The process conditions of the thermal sintering are: the heating rate is controlled at 10°C / min within 290°C, and the heating rate is controlled at 1°C / min in the range of 290-380°C; the temperature is kept at 380°C for 160-180min; during the cooling process, the temperature is within the range of 280-380°C, the cooling rate is controlled at 2°C / min, the temperature is kept at 300-320°C for 30-50min, and the rate in the remaining temperature sections is controlled at 5°C / min.

10. Use of the modified polytetrafluoroethylene according to any one of claims 1 to 7 in sealing products.

Citation Information

Cited By

  • Barium titanate-barite composite material as well as preparation method and application thereof

    CN119371183A