Smooth additive, etching solution, silicon wafer processing method, silicon wafer and solar cell

By using an etching solution of nitro-containing organic oxidants, hydrofluoric acid and water to replace the traditional pyramid smoothing process, the problem of increased reflectivity of silicon wafers is solved, the efficiency of solar cells is improved and the cost is reduced.

CN118853172APending Publication Date: 2024-10-29SONGSHAN LAKE MATERIALS LAB +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411042912.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing pyramid smoothing process causes the pyramid angle of the silicon wafer to change during the etching process, and the reflectivity increases significantly, which affects the photoelectric conversion efficiency of the solar cell. Traditional alternative processes such as ozone, hypochlorous acid, hydrogen peroxide, etc. have not been able to effectively solve this problem. question.

Method used

A sleek additive is used, including organic oxidant and water as the main components, and nitro-containing organic matter as the oxidant, replacing nitric acid in the traditional process. The etching conditions are controlled by combining hydrofluoric acid and water in the etching solution with the organic oxidant. In order to achieve a smooth treatment on the spire, reduce the oxidation of the side walls of the pyramid and reduce the reflectivity.

Benefits of technology

It effectively reduces the increase in reflectivity after silicon wafer smoothing, improves the photoelectric conversion efficiency of solar cells, and reduces raw material and wastewater treatment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118853172A_ABST
    Figure CN118853172A_ABST
Patent Text Reader

Abstract

The invention relates to a smoothing additive, an etching solution, a silicon wafer processing method, a silicon wafer and a solar cell, the smoothing additive comprises an organic oxidant and a first solvent, the organic oxidant comprises a nitro-containing organic matter, and the first solvent comprises water. The smoothing additive can replace nitric acid in the traditional pyramid smoothing process, and compared with the traditional process, the problem of increase of reflectivity before and after smoothing treatment is greatly improved, so that the photoelectric conversion efficiency of the solar cell is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular to a smoothing additive, an etching solution, a silicon wafer processing method, a silicon wafer and a solar cell. Background Art

[0002] At present, crystalline silicon solar cells have designed a variety of cell structures in pursuit of higher conversion efficiency, among which heterojunction cells have become the new generation of efficiency record holders. One of the reasons why heterojunction cells can achieve high efficiency is that they have excellent interface passivation, that is, a high minority carrier lifetime, which will help the cell obtain a higher open circuit voltage. The excellent passivation effect of heterojunction cells is due to the deposition of high-quality amorphous silicon / microcrystalline silicon passivation layers on the one hand, and on the other hand, it is also related to the special rounding treatment of its velvet structure. The rounded spire is conducive to the conformal deposition of subsequent thin films.

[0003] The pyramid rounding process commonly used on the current production line is to use a mixed solution of hydrofluoric acid and nitric acid to etch the textured silicon wafer. During the etching process, nitric acid oxidizes the silicon surface, and hydrofluoric acid dissolves the resulting silicon oxide. Since acid etching is isotropic, the protruding spires gradually become smooth. However, there is a problem with this process. Since the side walls of the pyramid will also be etched during the process, the angle of the pyramid will change, and the reflectivity will increase significantly, affecting the photoelectric conversion efficiency of the solar cell. In addition, some smoothing processes have been proposed, such as using ozone, hypochlorous acid, hydrogen peroxide, and chlorine as oxidants in conjunction with hydrofluoric acid, but these processes still cannot solve the problem of increased reflectivity. Summary of the invention

[0004] Based on this, it is necessary to provide a rounding additive, an etching solution, a silicon wafer processing method, a silicon wafer and a solar cell. The rounding additive can replace nitric acid in the traditional pyramid rounding process, and compared with the traditional process, the problem of increased reflectivity before and after the rounding process has been greatly improved, so that the photoelectric conversion efficiency of the solar cell has been effectively improved.

[0005] In a first aspect of the present application, a rounding additive is provided, comprising an organic oxidant and a first solvent, wherein the organic oxidant comprises a nitro-containing organic substance, and the first solvent comprises water.

[0006] In some embodiments, the content of the organic oxidant in the roundness additive is 1%-20% by mass.

[0007] In some embodiments, the content of the first solvent in the roundness additive is 80%-99% by mass.

[0008] In some embodiments, the content of the organic oxidant in the roundness additive is 7%-13% by mass.

[0009] In some embodiments, the content of the first solvent in the roundness additive is 87%-93% by mass.

[0010] In some embodiments, the nitro-containing organic compound includes one or more of o-nitroaniline, m-nitroaniline, p-nitroaniline, sodium o-nitrophenolate, sodium p-nitrophenolate, sodium 5-nitro-o-methoxyphenolate, 4-nitrocatechol, 4,5-dinitrocatechol and 4-(4-nitrophenylazo)catechol.

[0011] According to a second aspect of the present application, an etching solution is provided, comprising the rounding additive according to the first aspect of the present application, hydrofluoric acid, and a second solvent, wherein the second solvent comprises water.

[0012] In some embodiments, the mass percentages of the components in the etching solution are as follows: 0.1%-10% of the rounding additive, 0.1%-10% of the hydrofluoric acid, and 80%-98.8% of the second solvent.

[0013] The third aspect of the present application provides a silicon wafer processing method, comprising the step of placing a silicon wafer with a velvet surface in an etching solution for etching, wherein the etching solution comprises the smoothing additive described in the first aspect of the present application, hydrofluoric acid and a second solvent, and the second solvent comprises water.

[0014] In some embodiments, the mass percentages of the components in the etching solution are as follows: 0.1%-10% of the rounding additive, 0.1%-10% of the hydrofluoric acid, and 80%-98.8% of the second solvent.

[0015] In some embodiments, the process conditions of the etching treatment include: an etching temperature of 15° C.-90° C., and an etching time of 60 s-1200 s.

[0016] A fourth aspect of the present application provides a silicon wafer obtained by using the silicon wafer processing method described in the third aspect of the present application.

[0017] A fifth aspect of the present application provides a solar cell, comprising the silicon wafer described in the fourth aspect of the present application.

[0018] Compared with traditional technologies, the above-mentioned smooth additives have at least the following advantages:

[0019] The organic oxidant in the above-mentioned rounding additive includes organic matter containing nitro groups. Since the oxidizing property of nitro groups is sufficient to oxidize silicon, and the stability is better than that of organic matter containing peroxide groups, and the oxidizing property of nitro groups in organic matter is weaker than that of inorganic oxidants such as nitric acid, ozone, and hydrogen peroxide, the organic oxidant mainly oxidizes the top of the pyramid where the energy barrier required for oxidation is lower, and oxidizes the side walls of the pyramid less, so that hydrofluoric acid etching mainly occurs at the top of the pyramid of the texturing silicon wafer, achieving almost no increase in reflectivity before and after the rounding treatment, thereby improving the photoelectric conversion efficiency of solar cells. In addition, the above-mentioned rounding additive can replace nitric acid in the traditional pyramid rounding process. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the SEM surface structure image of the textured silicon wafer before rounding treatment in Example 1.

[0021] Figure 2 This is the SEM cross-sectional structure diagram of the textured silicon wafer before rounding treatment in Example 1.

[0022] Figure 3 This is the SEM surface structure image of the textured silicon wafer after the rounding treatment in Example 1.

[0023] Figure 4 This is the SEM cross-sectional structure diagram of the textured silicon wafer after the rounding treatment in Example 1. DETAILED DESCRIPTION

[0024] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0025] In this application, "first aspect", "second aspect", "third aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0026] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0027] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0028] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0029] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by technicians in the technical field of this application. The terms used in this application and in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more related listed items. The term "multiple" in this application means at least two, such as two, three, etc., unless otherwise clearly and specifically limited.

[0030] An embodiment of the present application provides a rounding additive, comprising an organic oxidant and a first solvent, wherein the organic oxidant comprises a nitro-containing organic substance, and the first solvent comprises water.

[0031] Since the oxidizing property of nitro groups is sufficient to oxidize silicon, and the stability is better than that of organic matter containing peroxide, and the oxidizing property of nitro groups in organic matter is weaker than that of inorganic oxidants such as nitric acid, ozone, and hydrogen peroxide, the organic oxidants mainly oxidize the top of the pyramid where the energy barrier required for oxidation is lower, and the side walls of the pyramid are less oxidized, resulting in hydrofluoric acid etching mainly occurring at the top of the pyramid of the texturing silicon wafer, achieving almost no increase in reflectivity before and after the rounding treatment. Compared with the traditional process, the problem of increased reflectivity before and after the rounding treatment has been greatly improved, thereby effectively improving the photoelectric conversion efficiency of solar cells. In addition, the above-mentioned rounding additive can replace nitric acid in the traditional pyramid rounding process.

[0032] In some embodiments, the roundness additive consists of an organic oxidant and a first solvent. Optionally, the first solvent is water.

[0033] In some embodiments, the content of organic oxidant in the rounding additive is 1%-20% by mass. Such a design can not only achieve the expected etching amount at the right time, but also control the etching speed and etching time, which is beneficial to further reduce the reflectivity of the textured silicon wafer after rounding treatment, while further improving the photoelectric conversion efficiency of solar cells. It is understandable that the content of organic oxidant in the rounding additive includes but is not limited to: 1%, 2%, 4%, 7%, 8%, 10%, 13%, 15%, 18%, 20%. Further, the content of organic oxidant in the rounding additive is 7%-13% by mass.

[0034] In some embodiments, the content of the first solvent in the rounding additive is 80%-99% by mass. With such a design, the expected etching amount can be achieved at the appropriate time, and the etching speed and etching time can be controlled, which is beneficial to further reduce the reflectivity of the textured silicon wafer after the rounding treatment. It is understandable that the content of the first solvent in the rounding additive includes but is not limited to: 80%, 83%, 85%, 87%, 89%, 91%, 93%, 95%, 97%, 99%. Further, the content of the first solvent in the rounding additive is 87%-93% by mass.

[0035] In some embodiments, the nitro-containing organic compound includes one or more of o-nitroaniline, m-nitroaniline, p-nitroaniline, sodium o-nitrophenolate, sodium p-nitrophenolate, sodium 5-nitro-o-methoxyphenolate, 4-nitrocatechol, 4,5-dinitrocatechol and 4-(4-nitrophenylazo)catechol.

[0036] Another embodiment of the present application provides an etching solution, comprising the above-mentioned smoothing additive of the present application, hydrofluoric acid and a second solvent, wherein the second solvent comprises water.

[0037] In some embodiments, the mass percentage of each component in the etching solution is as follows: 0.1%-10% of rounding additive, 0.1%-10% of hydrofluoric acid, and 80%-98.8% of the second solvent. The rounding additive can replace the nitric acid in the traditional pyramid rounding process, with lower usage and lower wastewater treatment costs. The higher the content of the rounding additive, the faster the rate at which the pyramid reacts to generate silicon oxide, and the corresponding hydrofluoric acid content needs to be increased synchronously, otherwise the removal rate of silicon oxide is limited, resulting in further oxidation of the subsequent pyramid being limited. If the content of hydrofluoric acid has already matched the oxidation rate of the pyramid, further increasing the amount of hydrofluoric acid has little effect on the etching rate. It can be understood that the mass percentage of the smoothing additive in the etching solution includes but is not limited to: 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%; the mass percentage of hydrofluoric acid in the etching solution includes but is not limited to: 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%; the mass percentage of the second solvent in the etching solution includes but is not limited to: 80%, 82%, 84%, 86%, 88%, 90%, 92%, 94%, 96%, and 98.8%.

[0038] In addition, the mass content of the organic oxidant in the etching solution in the above embodiment is much lower than the mass content of nitric acid in the traditional pyramid rounding process (generally 50%-80%), which can effectively reduce the cost of raw materials and wastewater treatment costs.

[0039] In some embodiments, the second solvent is water.

[0040] In some embodiments, the method for preparing the etching solution comprises the following steps:

[0041] The above-mentioned smooth additive, hydrofluoric acid and the second solvent of the present application are mixed to obtain an etching solution.

[0042] Another embodiment of the present application provides a silicon wafer processing method, including the step of placing a silicon wafer with a velvet surface in an etching solution for etching, the etching solution including the above-mentioned smoothing additive of the present application, hydrofluoric acid and a second solvent, and the second solvent includes water.

[0043] Place the silicon wafer with a velvet surface in an etching solution for etching. After a certain period of reaction, a silicon wafer with a smooth pyramid top can be obtained.

[0044] In some embodiments, the mass percentage of each component in the etching solution is as follows: 0.1%-10% of rounding additive, 0.1%-10% of hydrofluoric acid, and 80%-98.8% of the second solvent. The rounding additive can replace the nitric acid in the traditional pyramid rounding process, with lower usage and lower wastewater treatment costs. The higher the content of the rounding additive, the faster the rate at which the pyramid reacts to generate silicon oxide, and the corresponding hydrofluoric acid content needs to be increased synchronously, otherwise the removal rate of silicon oxide is limited, resulting in further oxidation of the subsequent pyramid being limited. If the content of hydrofluoric acid has already matched the oxidation rate of the pyramid, further increasing the amount of hydrofluoric acid has little effect on the etching rate. It can be understood that the mass percentage of the smoothing additive in the etching solution includes but is not limited to: 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%; the mass percentage of hydrofluoric acid in the etching solution includes but is not limited to: 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%; the mass percentage of the second solvent in the etching solution includes but is not limited to: 80%, 82%, 84%, 86%, 88%, 90%, 92%, 94%, 96%, and 98.8%.

[0045] In some embodiments, the process conditions of the etching treatment include: an etching temperature of 15°C-90°C, and an etching time of 60s-1200s. The higher the etching temperature, the faster the etching rate, which can reduce the etching time or the amount of the tower tip smoothing additive in the etching solution accordingly. It can be understood that the etching temperature includes but is not limited to: 15°C, 25°C, 35°C, 45°C, 55°C, 65°C, 75°C, 85°C, 90°C; the etching time includes but is not limited to: 60s, 120s, 180s, 240s, 360s, 420s, 500s, 600s, 700s, 800s, 900s, 1000s, 1100s, 1200s.

[0046] Another embodiment of the present application also provides a silicon wafer, which is obtained by the silicon wafer processing method of the present application. It can be understood that the silicon wafer with a velvet surface refers to a velvet-made silicon wafer, and the above silicon wafer includes a silicon wafer for a solar cell.

[0047] Another embodiment of the present application further provides a solar cell, comprising the silicon wafer mentioned above.

[0048] Another embodiment of the present application further provides an electrical device, including the solar cell of the present application. The electrical device may include mobile devices, such as mobile phones, laptop computers, etc., electric vehicles, electric trains, ships and satellites, power generation systems, etc., but is not limited thereto.

[0049] In order to further illustrate the present application, the technical scheme of the present application is described in detail below in conjunction with specific examples. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in the field or the product instructions are used. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0050] Example 1

[0051] (1) Add 100 g of an organic oxidant to deionized water (the first solvent) to prepare a 1000 g mixed solution and stir evenly to obtain a rounding additive for the top of a pyramid of a texturing silicon wafer; by mass percentage, the content of the organic oxidant in the rounding additive is 10%, and the content of the first solvent in the rounding additive is 90%;

[0052] The organic oxidant is sodium 5-nitro-o-methoxyphenol;

[0053] (2) mixing the tower tip smoothing additive obtained in step (1) in a formula of 5% tower tip smoothing additive, 1% hydrofluoric acid, and the remainder deionized water (second solvent) to obtain an etching solution;

[0054] (3) Immerse the cleaned silicon wafer with a velvet surface in the etching solution obtained in step (2) for reactive etching at a temperature of 25° C. for 300 s to obtain a silicon wafer with a smooth pyramid tip.

[0055] Example 2

[0056] (1) adding 80 g of an organic oxidant to deionized water (the first solvent) to prepare a 1000 g mixed solution and stirring the solution to obtain a rounding additive for the top of a pyramid of a texturing silicon wafer; by mass percentage, the content of the organic oxidant in the rounding additive is 8%, and the content of the first solvent in the rounding additive is 92%;

[0057] The organic oxidant consists of 40 g of sodium 5-nitro-o-methoxyphenol and 40 g of sodium p-nitrophenol;

[0058] (2) mixing the tower tip smoothing additive obtained in step (1) in a formula of 2.5% of the tower tip smoothing additive, 1% of hydrofluoric acid, and the remainder of deionized water (second solvent) to obtain an etching solution;

[0059] (3) Immerse the cleaned silicon wafer with a velvet surface in the etching solution obtained in step (2) for reactive etching at a temperature of 25° C. for 200 s to obtain a silicon wafer with a smooth pyramid tip.

[0060] Example 3

[0061] (1) Add 120 g of an organic oxidant to deionized water (the first solvent) to prepare a 1000 g mixed solution and stir evenly to obtain a rounding additive for the top of a pyramid of a texturing silicon wafer; by mass percentage, the content of the organic oxidant in the rounding additive is 12%, and the content of the first solvent in the rounding additive is 88%;

[0062] The organic oxidant is sodium o-nitrophenolate;

[0063] (2) mixing the tower tip smoothing additive obtained in step (1) in a formula of 7% tower tip smoothing additive, 2% hydrofluoric acid, and the remainder deionized water (second solvent) to obtain an etching solution;

[0064] (3) Immerse the cleaned silicon wafer with a velvet surface in the etching solution obtained in step (2) for reactive etching at an etching temperature of 25° C. for an etching time of 500 s to obtain a silicon wafer with a smooth pyramid top.

[0065] Example 4

[0066] (1) Add 10 g of an organic oxidant to deionized water (the first solvent) to prepare a 1000 g mixed solution and stir evenly to obtain a rounding additive for the top of a pyramid of a texturing silicon wafer; by mass percentage, the content of the organic oxidant in the rounding additive is 1%, and the content of the first solvent in the rounding additive is 99%;

[0067] The organic oxidant is sodium 5-nitro-o-methoxyphenol;

[0068] (2) mixing the tower tip smoothing additive obtained in step (1) in a formula of 5% tower tip smoothing additive, 1% hydrofluoric acid, and the remainder deionized water (second solvent) to obtain an etching solution;

[0069] (3) Immerse the cleaned silicon wafer with a velvet surface in the etching solution obtained in step (2) for reactive etching at a temperature of 25° C. for 300 s to obtain a silicon wafer with a smooth pyramid tip.

[0070] Example 5

[0071] (1) Add 70 g of an organic oxidant to deionized water (the first solvent) to prepare a 1000 g mixed solution and stir evenly to obtain a rounding additive for the top of a pyramid of a texturing silicon wafer; by mass percentage, the content of the organic oxidant in the rounding additive is 7%, and the content of the first solvent in the rounding additive is 93%;

[0072] The organic oxidant is sodium 5-nitro-o-methoxyphenol;

[0073] (2) mixing the tower tip smoothing additive obtained in step (1) in a formula of 5% tower tip smoothing additive, 1% hydrofluoric acid, and the remainder deionized water (second solvent) to obtain an etching solution;

[0074] (3) Immerse the cleaned silicon wafer with a velvet surface in the etching solution obtained in step (2) for reactive etching at a temperature of 25° C. for 300 s to obtain a silicon wafer with a smooth pyramid tip.

[0075] Example 6

[0076] (1) Add 130 g of an organic oxidant to deionized water (the first solvent) to prepare a 1000 g mixed solution and stir evenly to obtain a rounding additive for the top of a pyramid of a texturing silicon wafer; by mass percentage, the content of the organic oxidant in the rounding additive is 13%, and the content of the first solvent in the rounding additive is 87%;

[0077] The organic oxidant is sodium 5-nitro-o-methoxyphenol;

[0078] (2) mixing the tower tip smoothing additive obtained in step (1) in a formula of 5% tower tip smoothing additive, 1% hydrofluoric acid, and the remainder deionized water (second solvent) to obtain an etching solution;

[0079] (3) Immerse the cleaned silicon wafer with a velvet surface in the etching solution obtained in step (2) for reactive etching at a temperature of 25° C. for 300 s to obtain a silicon wafer with a smooth pyramid tip.

[0080] Example 7

[0081] (1) Add 200 g of an organic oxidant to deionized water (the first solvent) to prepare a 1000 g mixed solution and stir evenly to obtain a rounding additive for the top of a pyramid of a texturing silicon wafer; by mass percentage, the content of the organic oxidant in the rounding additive is 20%, and the content of the first solvent in the rounding additive is 80%;

[0082] The organic oxidant is sodium 5-nitro-o-methoxyphenol;

[0083] (2) mixing the tower tip smoothing additive obtained in step (1) in a formula of 5% tower tip smoothing additive, 1% hydrofluoric acid, and the remainder deionized water (second solvent) to obtain an etching solution;

[0084] (3) Immerse the cleaned silicon wafer with a velvet surface in the etching solution obtained in step (2) for reactive etching at a temperature of 25° C. for 300 s to obtain a silicon wafer with a smooth pyramid tip.

[0085] Comparative Example 1

[0086] (1) Mix 70% nitric acid, 1% hydrofluoric acid, and the rest deionized water (second solvent) to obtain an etching solution;

[0087] (2) Immerse the cleaned silicon wafer with a velvet surface in the etching solution obtained in step (1) for reactive etching at a temperature of 25° C. for 90 seconds to obtain a silicon wafer with a smooth pyramid tip.

[0088] Test Case

[0089] The reflectivity test method of the texturing silicon wafer before and after rounding is as follows: Use a reflectivity tester (model: Zhidong Optoelectronics D8 reflectometer) to test the reflectivity of the texturing silicon wafer before and after rounding. During the test, place the silicon wafer flat on the test platform of the tester, and set the test wavelength range to 350nm~1050nm. Each time, 9 points on the silicon wafer are tested, and the average value is taken to obtain the reflectivity of the silicon wafer.

[0090] The reflectivity test results of the texturing silicon wafers before and after the rounding treatment in each embodiment and comparative example are shown in Table 1.

[0091] Table 1

[0092]

[0093] Depend on Figure 1-Figure 4 It can be seen that the SEM surface and SEM cross section of the textured silicon wafer after rounding treatment in Example 1 are compared with those before rounding, the pyramid top becomes smoother, and the side wall of the pyramid does not change much. From the data in Table 1, it can be seen that compared with Comparative Example 1, the reflectivity increase of the textured silicon wafers of Examples 1-7 after rounding treatment is relatively small, indicating that the use of the rounding additives of Examples 1-7 of the present application can effectively improve the problem of the increase in reflectivity of the textured silicon wafer after rounding treatment, thereby effectively improving the photoelectric conversion efficiency of the solar cell.

[0094] Compared with Example 1 and Examples 5-6, the rise of the texturized silicon wafer in Example 4 after rounding treatment is not large, which is caused by the lack of obvious rounding. The structure that has not been smoothed is not conducive to the solar cell to obtain a higher photoelectric conversion efficiency. The rise of the texturized silicon wafer in Example 7 after rounding treatment is larger, which is due to excessive rounding, so the reflectivity increases more. Example 1 and Examples 5-6 can maintain sufficient rounding effect and reduce the reflectivity after smoothing, so the photoelectric conversion efficiency of the solar cell can be further improved.

[0095] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0096] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims, and the description may be used to interpret the content of the claims.

Claims

1. A smooth additive, It is characterized in that The method comprises an organic oxidant and a first solvent, wherein the organic oxidant comprises an organic substance containing a nitro group, and the first solvent comprises water.

2. The roundness additive according to claim 1, It is characterized in that The roundness additive has at least one of the following characteristics (1)-(2): (1) The content of the organic oxidant in the roundness additive is 1%-20% by mass; (2) Calculated by mass percentage, the content of the first solvent in the roundness additive is 80%-99%.

3. The roundness additive according to claim 2, It is characterized in that The roundness additive has at least one of the following characteristics (1)-(2): (1) The content of the organic oxidant in the roundness additive is 7%-13% by mass percentage; (2) Calculated by mass percentage, the content of the first solvent in the roundness additive is 87%-93%.

4. The roundness additive according to any one of claims 1 to 3, It is characterized in that The nitro-containing organic matter includes one or more of o-nitroaniline, m-nitroaniline, p-nitroaniline, sodium o-nitrophenolate, sodium p-nitrophenolate, sodium 5-nitro-o-methoxyphenolate, 4-nitrocatechol, 4,5-dinitrocatechol and 4-(4-nitrophenylazo)catechol.

5. An etching solution, It is characterized in that The method comprises the rounding additive according to any one of claims 1 to 4, hydrofluoric acid and a second solvent, wherein the second solvent comprises water.

6. The etching solution according to claim 5, It is characterized in that The mass percentages of the components in the etching solution are as follows: 0.1%-10% of the rounding additive, 0.1%-10% of the hydrofluoric acid, and 80%-98.8% of the second solvent.

7. A silicon wafer processing method, It is characterized in that The method comprises the step of placing a silicon wafer with a velvet surface in an etching solution for etching, wherein the etching solution comprises the rounding additive according to any one of claims 1 to 4, hydrofluoric acid and a second solvent, and the second solvent comprises water.

8. The silicon wafer processing method according to claim 7, It is characterized in that The mass percentages of the components in the etching solution are as follows: 0.1%-10% of the rounding additive, 0.1%-10% of the hydrofluoric acid, and 80%-98.8% of the second solvent; Optionally, the process conditions of the etching treatment include: an etching temperature of 15° C.-90° C., and an etching time of 60s-1200s.

9. A silicon wafer, It is characterized in that The method is obtained by using the silicon wafer processing method described in any one of claims 7-8.

10. A solar cell, It is characterized in that Including the silicon wafer as claimed in claim 9.