Catalyst slurry as well as preparation method and application thereof
Through two dispersion steps and the use of surfactants, a double-layer structure of the catalyst slurry is constructed, which solves the problems of membrane electrode structure disorder and catalyst instability, and improves the performance and durability of the membrane electrode.
Patent Information
- Application Number
- CN202410827903.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-29
AI Technical Summary
The existing catalyst slurry preparation method involves single-step feeding, mixing and dispersion, which results in a chaotic membrane electrode structure and is not conducive to drainage. The point-to-point contact between the catalyst and the perfluorosulfonic acid resin cannot ensure sufficient oxygen reduction reaction sites and the stability of Pt particles. exists, resulting in low membrane electrode performance and poor durability.
Using a two-step dispersion method, firstly form a primary dispersion of catalysts continuously coated with resin through high-energy dispersion, then adjust the distribution of ionomers in low-energy dispersion, and use surfactants to improve the dispersion and stability of the catalyst to construct a double dispersion. The layer-structured proton channel and gas-liquid transmission channel optimize coating cracks and overall performance.
It improves the water vapor transmission path of the membrane electrode, optimizes the coating effect, improves the dispersion and stability of the catalyst, enhances the oxygen reduction reaction capacity and the durability of the membrane electrode, and improves the overall performance.
Smart Images

Figure CN118867271A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a catalyst slurry and a preparation method and application thereof. Background Art
[0002] Proton exchange membrane fuel cell (PEMFC) is an energy conversion device that can directly convert chemical energy into electrical energy. It basically does not emit greenhouse gases during the conversion process, which can effectively mitigate the greenhouse effect. At the same time, it is not limited by the Carlo cycle and has a higher conversion efficiency than traditional internal combustion engines. In theory, the conversion efficiency of fuel cells can reach 90%, and in practical applications it can reach 60%. In addition, it also has the advantages of being green, environmentally friendly, zero-emission and sustainable, and has become the key to solving energy crises and environmental problems.
[0003] Membrane electrode (MEA) is the core component of PEMFC. Its cathode and anode have oxygen reduction reaction (ORR) and hydrogen oxidation reaction (HOR) respectively. These reactions determine the energy conversion capacity of the fuel cell. The membrane electrode is mainly composed of three parts, namely polymer membrane, catalyst layer and gas diffusion layer. The preparation method of the cathode catalyst layer has an important influence on its microstructure. A reasonable structure can enable the cathode catalyst layer to quickly transfer oxygen to the reaction active site and quickly discharge the water produced by the reaction. It can be seen that constructing the ideal three-dimensional morphology and network structure of clusters in the catalyst slurry is a key difficulty to be solved.
[0004] In current traditional industrial production, the preparation of catalyst slurry is usually a single-step process of adding materials, mixing and dispersing. The membrane electrode structure formed by coating is chaotic, which is not conducive to drainage. At the same time, the point-to-point contact between the catalyst and the perfluorosulfonic acid resin cannot guarantee sufficient oxygen reduction reaction sites during the battery operation process and the stable existence of Pt particles, resulting in low membrane electrode performance and poor durability.
[0005] In different solvent systems, the ionomer perfluorosulfonic acid resin will exist in different structures such as granules, rods or large agglomerates. As the concentration of the ionomer increases, the ionomer begins to agglomerate. In the slurry, these ionomers will spontaneously adsorb on the catalyst in different forms. However, these ionomers are not uniformly or all adsorbed on the ionomer, but exist in the form of point contact with the catalyst. At the same time, the ionomer adsorption rate is also greatly affected by the polarity of the solvent system. If the ionomer covers the catalyst too thickly or the ionomer does not contact the catalyst, the following results will occur: 1. The redox reaction is reduced or the three-phase interface is reduced; 2. The resistance to proton conduction and water vapor transmission increases; 3. The carbon frame collapses and the Pt particles fall off. Summary of the invention
[0006] The present invention provides a catalyst slurry and a preparation method and application thereof, so as to solve the problems that the preparation of the existing membrane electrode catalyst slurry is usually a single-step process of adding materials, mixing and dispersing, the membrane electrode structure formed by coating is chaotic and not conducive to drainage, and the point-to-point contact between the catalyst and the perfluorosulfonic acid resin cannot ensure sufficient oxygen reduction reaction sites during the battery operation process and the stable existence of Pt particles, resulting in low membrane electrode performance and poor durability.
[0007] The present invention provides a method for preparing a catalyst slurry, comprising the following steps: Step (1): high-energy dispersing, drying and grinding the catalyst, partially perfluorosulfonic acid resin, surfactant and first solvent to obtain a primary dispersion of the catalyst continuously coated with the resin; Step (2): low-energy dispersion is performed on the obtained catalyst primary dispersion, the remaining part of the perfluorosulfonic acid resin and the second solvent to obtain a catalyst slurry; wherein the alcohol-water ratio of the second solvent is less than the alcohol-water ratio of the first solvent.
[0008] In the above scheme, a method for preparing a catalyst slurry of the present invention adds a surfactant, utilizes the rapid dissolution of the surfactant in the solvent to generate surface tension to help the catalyst particles to be highly dispersed, and adds the ionomer perfluorosulfonic acid resin twice in a solvent environment with different alcohol-water ratios, utilizes the different polarities and different strengths of different solvent systems to orderly regulate the catalyst dispersibility, stability and distribution regularity of the ionomer perfluorosulfonic acid resin, constructs a double-layer proton channel and transmission channel, and forms a highly regular distribution structure that is superior to traditional point-to-point proton transmission channels and single-scale gas-liquid transmission channels, forming a water vapor transmission path that is small and dense inside and large and loose outside, which is beneficial to improving the problem of water flooding during operation and optimizing coating cracks and overall performance.
[0009] Specifically, the preparation method of the present invention includes two dispersion steps, which have different purposes but cooperate with each other and work synergistically. The main purpose of the first dispersion step is to disperse the catalyst efficiently. On the one hand, the polarity of the solvent system with a high alcohol-water ratio is relatively small, and the attraction effect with the hydrophobic carbon-fluorine main chain in the ionomer is increased. Therefore, during the dispersion process, the polymer chain provides a pulling force to the catalyst particles, which helps the dispersion of the particles; at the same time, the polymer ionomer causes the surface potential of the carbon-based platinum particles to change, which also increases the electrostatic effect and spatial repulsion between the particles, which plays an important role in the dispersibility of the ink. On the other hand, in an environment with a high alcohol-water ratio, the resin will exist in a small, flexible, and dense ring-shaped form of about 30nm, and the smaller form can smoothly contact the surface of the Pt-C particles; at the same time, the surface fluorination of the added surfactant can generate electrostatic attraction with the first layer of perfluorosulfonic acid resin, so that it is evenly coated on the catalyst surface. In addition, further drying and grinding operations make it mixed at a smaller scale and generate electrostatic attraction, so that the thin layer of resin interface is in closer contact with the catalyst body, thereby forming a thin and continuous proton conduction surface network on the active surface of the catalyst. The main purpose of the second dispersion step is to adsorb and regulate the structure of the ionomer. As the water mass fraction increases, the hydrophilic solvent repels the hydrophobic carbon-fluorine backbone of the second added ionomer, thereby effectively adsorbing to the surface of the catalyst primary dispersion obtained in the first dispersion step. Different solvent systems have great differences in the effect on the structure of the catalyst slurry. The solubility parameter HSP-δP of the mixed solvent can be regulated by the Hansen equation. This parameter is an indicator of the solvent polarity and can effectively control the aggregate structure and viscoelastic property parameters of the catalyst slurry. The overall structure of the aggregate of the catalyst slurry finally prepared presents a double-layer structure with dense inside and sparse outside. At this time, the catalyst slurry presents a medium to low viscosity (30±10mpa·s) due to the high polarity dispersion environment.
[0010] Effectively improve the subsequent coating crack problem: In the subsequent coating process of the catalyst layer, the catalyst slurry formed by the present invention significantly optimizes the coating appearance and microscopic effects. The principle is: First, because the catalyst slurry contains less highly volatile alcohol solvents, the drying speed of the catalyst layer is reduced to a certain extent, which is conducive to reducing the generation of various types of cracks. Secondly, controlling the alcohol / water ratio in the slurry formula is quite beneficial to further adjust the surface tension of the droplets. The optimal surface tension of the solution to be coated is 5mN / m lower than that of the substrate, otherwise the solution will be difficult to spread evenly on the substrate, resulting in relatively poor coating quality. In addition, the microstructure of the catalyst layer to be formed during the coating process shows relatively loose reaction units, which is more conducive to the volatilization of the solvent.
[0011] In order to better improve the dispersibility and stability of the catalyst in the catalyst slurry, further, the surfactant includes one or more of alkyl sulfonic acid, aryl sulfonic acid, perfluoroalkyl sulfonic acid, perfluoroaryl sulfonic acid, alkyl sulfuric acid, aryl sulfuric acid, perfluoroalkyl sulfuric acid, perfluoroaryl sulfuric acid, alkyl carboxylic acid, aryl carboxylic acid, perfluoroalkyl carboxylic acid, perfluoroaryl carboxylic acid, alkyl phosphoric acid, aryl phosphoric acid, perfluoroalkyl phosphoric acid and perfluoroaryl phosphoric acid.
[0012] Preferably, the surfactant is selected from one or more of perfluoroalkyl sulfonic acid, perfluoroaryl sulfonic acid, perfluoroalkyl sulfuric acid, perfluoroaryl sulfuric acid, perfluoroalkyl carboxylic acid, perfluoroaryl carboxylic acid, perfluoroalkyl phosphoric acid and perfluoroaryl phosphoric acid.
[0013] In the above scheme, the surfactant is selected from perfluoro surfactants. The surface fluorination of the additive can generate electrostatic attraction with the first layer of perfluorosulfonic acid resin, so that it is evenly coated on the catalyst surface, thereby improving the dispersion and stability of the catalyst in the catalyst slurry.
[0014] More preferably, the surfactant is selected from one or more of perfluorooctane sulfonic acid, perfluorododecyl phosphoric acid, perfluorooctane carboxylic acid and perfluorododecyl sulfuric acid.
[0015] Furthermore, in the step (1), the weight ratio of the catalyst to the sum of the weight of the partial perfluorosulfonic acid resin and the surfactant is 1:1 to 3:1.
[0016] Optionally, the weight ratio of the catalyst to the sum of the weight of the partial perfluorosulfonic acid resin and the surfactant can be 1:1, 1.5:1, 2.5:1 or 3:1, etc., and of course can be other values within the above range, which is not limited here.
[0017] Furthermore, in the first solvent, the weight percentage of organic alcohol is ≥70%; in the second solvent, the weight percentage of organic alcohol is ≤50%.
[0018] Optionally, in the first solvent, the weight percentage of the organic alcohol can be 70%, 75%, 80%, 85%, 90% or 95%, etc., and of course it can also be other values within the above range, which is not limited here, and is preferably 70%-85%; in the second solvent, the weight percentage of the organic alcohol can be 45%, 40%, 35%, 30%, 25%, 20%, 15% or 10%, etc., and of course it can also be other values within the above range, which is not limited here, and is preferably 20%-50%.
[0019] Preferably, the organic alcohol in the first solvent and the second solvent each independently comprises one or more of n-propanol, isopropanol, ethanol, diacetone alcohol and propylene glycol; more preferably, the first solvent and the second solvent are different.
[0020] Furthermore, in the step (1), the weight percentage of the partial perfluorosulfonic acid resin used in the preparation process is ≤50% of the total weight of the perfluorosulfonic acid resin used.
[0021] In the above scheme, by limiting the weight percentage of the partial perfluorosulfonic acid resin used in the preparation process to a reasonable range, it is more conducive to regulating the catalyst dispersibility, stability and distribution regularity of the ionomer resin.
[0022] Furthermore, in step (1), the catalyst is selected from one or more of Pt / C, platinum black and Pt-Co / C.
[0023] In the above scheme, by selecting a suitable type of catalyst, the catalytic performance of the catalyst layer formed by the catalyst slurry can be improved.
[0024] Furthermore, the thickness of the catalyst primary dispersion is 0.01-0.1 μm.
[0025] Optionally, the thickness of the catalyst primary dispersion may be 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm or 0.1 μm, etc., and may also be other values within the above range, which is not limited here.
[0026] Furthermore, in step (1), the high-energy dispersion method includes ball milling, high-pressure homogenization or ultrasonic crushing. Furthermore, the ball milling parameters are rotation 300-400rpm, revolution 1-3rpm, temperature control 5-10°C, ball milling time 12-15 hours; high-pressure homogenization parameters are pressure 20000-40000psi, homogenization 4-6 times; ultrasonic crushing parameters are ultrasonic time 15-30 minutes; In the above scheme, by selecting a suitable high-energy dispersion method, it is more conducive to the efficient dispersion of the catalyst.
[0027] Furthermore, in the step (1), the drying temperature is greater than or equal to 60°C and less than or equal to 80°C.
[0028] Furthermore, in the step (2), the low-energy dispersion method includes high-speed shearing, and preferably, the rate of high-speed shearing is 1000-3000 rpm.
[0029] In the above scheme, by selecting a suitable low-energy dispersion method, it is more conducive to the adsorption and structural adjustment of the ionomer.
[0030] According to the second aspect of the present invention, the present invention further provides a catalyst slurry prepared by the above-mentioned preparation method; preferably, the aggregate of the catalyst slurry presents a double-layer structure with dense inner layer and sparse outer layer; the viscosity of the catalyst slurry is 20-40mpa·s; the particle size distribution of the catalyst slurry is D90<3μm, D50<1μm; preferably, D90<1μm, D50<0.5μm; more preferably, 1.5≤(Dv90-Dv10) / Dv50≤2
[0031] According to a third aspect of the present invention, the present invention also provides the use of the above-mentioned catalyst slurry in a membrane electrode, wherein the membrane electrode comprises a polymer membrane, a catalyst layer and a gas diffusion layer, and the catalyst layer is formed by the catalyst slurry.
[0032] The present invention provides a method for preparing a catalyst slurry, which adds an ionomer twice under different solvent environments, and utilizes different solvent systems with greatly different polarities and different dispersion strengths to orderly regulate the catalyst dispersibility, stability and distribution regularity of the ionomer resin, while optimizing coating cracks and overall performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 It is a diagram showing the wetted contact state of the membrane electrode catalyst slurry of Example 1 of the present invention and Comparative Example 1 on PTFE.
[0035] Figure 2 It is a surface state diagram of the membrane layer prepared by the membrane electrode catalyst slurry of Example 1 of the present invention and Comparative Example 1.
[0036] Figure 3 It is a polarization performance curve diagram of the membrane electrode made of the membrane electrode catalyst slurry of Example 15 of the present invention and Comparative Example 1.
[0037] Figure 4 This is a particle size distribution diagram of the membrane electrode catalyst slurry of Example 1 of the present invention. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] In the following examples, the catalyst is selected from Umicore 0550, the perfluorosulfonic acid resin is selected from Solvay D79, and the solid content is 25%wt.
[0040] Example 1
[0041] This embodiment provides a method for preparing a membrane electrode catalyst slurry, comprising the following steps: Step (1): 2 g of catalyst, 1 g of the first part of perfluorosulfonic acid resin, 7 g of n-propanol, 3 g of ultrapure water, and 1 g of surfactant perfluorooctane sulfonic acid are dispersed by ball milling (ball milling dispersion is 350 rpm rotation, 2 rpm revolution, temperature control 8°C, ball milling time 14 hours), and the obtained slurry is dried and ground in an environment of 60°C to obtain a primary dispersion of the catalyst wrapped by the perfluorosulfonic acid resin (thickness 1.5 μm), and the first layer of resin exists in a small and dense form.
[0042] The first part of the perfluorosulfonic acid resin accounts for 50% of the total weight of the perfluorosulfonic acid resin used in the preparation method, the ratio of catalyst / (the first part of the perfluorosulfonic acid resin+surfactant) is 1:1, and the ratio of alcohol in the solvent system (n-propanol+ultrapure water) is 70%.
[0043] Step (2): Weigh 14 g of the above-prepared catalyst primary dispersion, 1 g of the second part of perfluorosulfonic acid resin, 2 g of propylene glycol, and 15 g of ultrapure water (the proportion of alcohol in the solvent system is 45%) and perform high-speed shearing at a speed of 2000r to obtain a catalyst slurry for coating, in which the resin exists in a large and loose form.
[0044] Example 2
[0045] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from Embodiment 1 in that: in step (1), the amount of catalyst is changed so that the ratio of catalyst / (first part of perfluorosulfonic acid resin+surfactant) is 2:1.
[0046] Example 3
[0047] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from Embodiment 1 in that: in step (1), the amount of catalyst is changed so that the ratio of catalyst / (first part of perfluorosulfonic acid resin+surfactant) is 3:1.
[0048] Example 4
[0049] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from Embodiment 1 in that: in step (1), the amount of catalyst is changed so that the ratio of catalyst / (first part of perfluorosulfonic acid resin+surfactant) is 0.5:1.
[0050] Example 5
[0051] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from Embodiment 1 in that: in step (1), the amount of catalyst is changed so that the ratio of catalyst / (first part of perfluorosulfonic acid resin+surfactant) is 3.5:1.
[0052] Example 6
[0053] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from Embodiment 1 in that: in step (1), the surfactant is perfluorododecanesulfuric acid.
[0054] Example 7
[0055] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that: in step (1), the surfactant is perfluorooctane carboxylic acid.
[0056] Example 8
[0057] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that: in step (1), the surfactant is perfluorododecyl phosphoric acid.
[0058] Example 9
[0059] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that: in step (1), the amount of alcohol is changed so that the proportion of alcohol in the solution system is 80%.
[0060] Example 10
[0061] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that: in step (1), the amount of alcohol is changed so that the proportion of alcohol in the solution system is 85%.
[0062] Embodiment 11
[0063] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that: in step (1), the amount of alcohol is changed so that the proportion of alcohol in the solution system is 60%.
[0064] Example 12
[0065] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that: in step (2), the amount of alcohol is changed so that the proportion of alcohol in the solution system is 30%.
[0066] Embodiment 13
[0067] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that: in step (2), the amount of alcohol is changed so that the proportion of alcohol in the solution system is 20%.
[0068] Embodiment 14
[0069] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that: in step (2), the amount of alcohol is changed so that the proportion of alcohol in the solution system is 15%.
[0070] Embodiment 15
[0071] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that: in step (2), the amount of alcohol is changed so that the proportion of alcohol in the solution system is 50%.
[0072] Example 16
[0073] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that: in step (1), the first part of the perfluorosulfonic acid resin accounts for 40% of the total weight of the perfluorosulfonic acid resin used in the preparation method.
[0074] Embodiment 17
[0075] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that: in step (1), the first part of the perfluorosulfonic acid resin accounts for 35% of the total weight of the perfluorosulfonic acid resin used in the preparation method.
[0076] Embodiment 18
[0077] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that: in step (1), the first part of the perfluorosulfonic acid resin accounts for 45% of the total weight of the perfluorosulfonic acid resin used in the preparation method.
[0078] Embodiment 19
[0079] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that: in step (1), an equal amount of isopropanol is used instead of n-propanol.
[0080] Embodiment 20
[0081] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from that of Embodiment 1 in that in step (1), an equal amount of ethanol is used instead of n-propanol.
[0082] Embodiment 21
[0083] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from Embodiment 1 in that in step (2), an equal amount of diacetone alcohol is used instead of propylene glycol.
[0084] Embodiment 22
[0085] This embodiment provides a method for preparing a membrane electrode catalyst slurry, which is different from Embodiment 1 in that: in step (1), an equal amount of isopropanol is used to replace n-propanol, and in step (2), an equal amount of isopropanol is used to replace propylene glycol.
[0086] Comparative Example 1
[0087] This comparative example provides a method for preparing a membrane electrode catalyst slurry, which is different from Example 1 in that: in step (1), no surfactant is added.
[0088] Comparative Example 2
[0089] This comparative example provides a method for preparing a membrane electrode catalyst slurry, which is different from Example 1 in that in step (1) and step (2), the proportion of alcohol in the solution system is 45%.
[0090] The catalyst slurry prepared in the examples and comparative examples was used to prepare CCM by blade coating. The PEM used was Gore enhanced 8 μm, with a cathode loading of 0.2 mg / cm 2 , anode loading 0.05mg / cm 2 , Carbon paper is Toray 055, active area 7*7cm 2 The prepared membrane electrode was tested for performance at a temperature of 85°C, a metering ratio of 2:3, a back pressure of 170 kPa / 150 kPa, and a humidity of 100%. The test results are shown in Table 1 below.
[0091] Table 1 Peak Power Example 1 1.845 Example 2 1.757 Example 3 1.704 Example 4 1.814 Example 5 1.684 Example 6 1.785 Example 7 1.824 Example 8 1.854 Example 9 1.884 Example 10 1.905 Embodiment 11 1.763 Example 12 1.724 Embodiment 13 1.705 Embodiment 14 1.668 Embodiment 15 1.914 Example 16 1.832 Embodiment 17 1.795 Embodiment 18 1.840 Embodiment 19 1.856 Embodiment 20 1.784 Embodiment 21 1.654 Embodiment 22 1.844 Comparative Example 1 1.452 Comparative Example 2 1.645
[0092] It can be seen from the experimental data in Table 1 that the preparation method of the present invention helps to highly disperse the catalyst particles by adding a surfactant and utilizing the rapid dissolution of the surfactant in the solvent to generate surface tension, and by adding the ionomer perfluorosulfonic acid resin twice in a solvent environment with different alcohol-water ratios, and utilizing the different polarities and different strengths of different solvent systems to orderly regulate the catalyst dispersibility, stability and distribution regularity of the ionomer perfluorosulfonic acid resin, so that the obtained membrane electrode catalyst slurry has excellent electrode performance.
[0093] The membrane electrode catalyst slurry of Example 1 and Comparative Example 1 was tested for surface tension using the hanging drop method. The test results are as follows: Figure 1 As shown, it can be seen that the contact angle of the membrane electrode catalyst slurry of Comparative Example 1 on PTFE is 113°, and the contact angle of the membrane electrode catalyst slurry of Example 1 on PTFE is 87°.
[0094] The membrane electrode catalyst slurry of Example 1 and Comparative Example 1 is coated on the high-temperature membrane cloth and dried. Figure 2 As shown, it can be seen that the film layer formed by the membrane electrode catalyst slurry of the present invention is flat and has no cracks, while the film layer formed by the membrane electrode catalyst slurry of Comparative Example 1 has obvious cracks.
[0095] The membrane electrode formed by the membrane electrode catalyst slurry of Example 15 and Comparative Example 1 was subjected to polarization performance test. The test method was 85°C, the metering ratio was 2:3, the back pressure was 170kPa / 150kPa, and the humidity was 100%. The test results are as follows Figure 3 As shown, it can be seen that the polarization curve performance of Example 15 is better than that of Comparative Example 1.
[0096] The catalyst slurry obtained in Example 1 was tested by electron microscope. It can be seen that the aggregates of the catalyst slurry present a double-layer structure with dense inner layer and sparse outer layer. The viscosity of the obtained catalyst slurry was tested. The viscosity was 34mpa·s. The particle size distribution of the obtained membrane electrode catalyst slurry was tested. The test results are as follows: Figure 4 As shown, it can be seen that Dv10 is 0.176 μm, Dv50 is 0.375 μm, Dv90 is 0.909 μm, the diameter distance = (Dv90-Dv10) / Dv50 = 1.954, and the particle size distribution meets the slurry preparation standard.
[0097] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a catalyst slurry, characterized in that: The steps include: Step (1): high-energy dispersing, drying and grinding the catalyst, partially perfluorosulfonic acid resin, surfactant and first solvent to obtain a primary dispersion of the catalyst continuously coated with the resin; Step (2): low-energy dispersion the obtained catalyst primary dispersion, the remaining part of the perfluorosulfonic acid resin and the second solvent to obtain a catalyst slurry; wherein the alcohol-water ratio of the second solvent is less than the alcohol-water ratio of the first solvent.
2. The method for preparing the catalyst slurry according to claim 1, characterized in that: The surfactant includes one or more of alkyl sulfonic acid, aryl sulfonic acid, perfluoroalkyl sulfonic acid, perfluoroaryl sulfonic acid, alkyl sulfuric acid, aryl sulfuric acid, perfluoroalkyl sulfuric acid, perfluoroaryl sulfuric acid, alkyl carboxylic acid, aryl carboxylic acid, perfluoroalkyl carboxylic acid, perfluoroaryl carboxylic acid, alkyl phosphoric acid, aryl phosphoric acid, perfluoroalkyl phosphoric acid and perfluoroaryl phosphoric acid; Preferably, the surfactant is selected from one or more of perfluoroalkyl sulfonic acid, perfluoroaryl sulfonic acid, perfluoroalkyl sulfuric acid, perfluoroaryl sulfuric acid, perfluoroalkyl carboxylic acid, perfluoroaryl carboxylic acid, perfluoroalkyl phosphoric acid and perfluoroaryl phosphoric acid; More preferably, the surfactant is selected from one or more of perfluorooctane sulfonic acid, perfluorododecyl phosphoric acid, perfluorooctane carboxylic acid and perfluorododecyl sulfuric acid.
3. The method for preparing the catalyst slurry according to claim 1, characterized in that: In the step (1), the weight ratio of the catalyst to the sum of the weight of the partial perfluorosulfonic acid resin and the surfactant is 1:1 to 3:
1.
4. The method for preparing the catalyst slurry according to claim 1, characterized in that: The weight percentage of organic alcohol in the first solvent is ≥70%; the weight percentage of organic alcohol in the second solvent is ≤50%; Preferably, the organic alcohol in the first solvent and the second solvent each independently comprises one or more of n-propanol, isopropanol, ethanol, diacetone alcohol and propylene glycol; more preferably, the first solvent and the second solvent are different.
5. The method for preparing the catalyst slurry according to claim 1, characterized in that: In the step (1), the weight percentage of the partial perfluorosulfonic acid resin used in the preparation process is ≤50% of the total weight of the perfluorosulfonic acid resin used.
6. The method for preparing the catalyst slurry according to claim 1, characterized in that: In the step (1), the catalyst is selected from one or more of Pt / C, platinum black and Pt-Co / C.
7. The method for preparing the catalyst slurry according to claim 1, characterized in that: The thickness of the catalyst primary dispersion is 0.01 to 0.1 μm.
8. The method for preparing the catalyst slurry according to claim 1, characterized in that: In the step (1), the high-energy dispersion method includes ball milling, high-pressure homogenization or ultrasonic crushing; And / or, in step (1), the drying temperature is greater than or equal to 60° C. and less than or equal to 80° C.; And / or, in step (2), the low-energy dispersion method includes high-speed shearing.
9. A catalyst slurry, characterized in that: The catalyst slurry is prepared by the preparation method according to any one of claims 1 to 8; preferably, the aggregates of the catalyst slurry present a double-layer structure with dense inner layer and sparse outer layer; the viscosity of the catalyst slurry is 20-40 mpa·s; the particle size distribution of the catalyst slurry is D90<3 μm, D50<1 μm.
10. Use of the catalyst slurry according to claim 9 in a membrane electrode, characterized in that: The membrane electrode comprises a polymer membrane, a catalyst layer and a gas diffusion layer, wherein the catalyst layer is formed by the catalyst slurry.
Citation Information
Cited By
Membrane electrode slurry preparation method and membrane electrode slurry
CN122382603A