Novel calcium-containing sulfonic acid type ionomer flame retardant as well as preparation method and application thereof

By developing calcium-containing sulfonic acid-containing ionomer flame retardant, the problem of poor compatibility between existing sulfonate flame retardant and polycarbonate is solved, and the high flame retardant effect and mechanical properties are improved under low addition amounts , suitable for applications with high safety requirements.

CN118878809AActive Publication Date: 2024-11-01ZHONGBEI UNIV

Patent Information

Application Number
CN202411128373.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-01
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The molecular structure of existing sulfonate flame retardants is too different from that of polycarbonate, resulting in poor compatibility of composite materials, reducing mechanical properties, and easily releasing smoke at high temperatures, limiting its application with high safety requirements. Use for occasions.

Method used

Develop a calcium-containing sulfonic acid-containing ionomer flame retardant with a chemical structure similar to that of polycarbonate. It undergoes sulfonation reaction by mixing polycarbonate with sulfonation reagents and ion exchange reaction with metal source modified components. , a flame retardant with good compatibility was prepared.

Benefits of technology

The high flame retardant effect is achieved at a lower addition amount, maintaining the high mechanical properties of the composite material, suitable for applications with high safety requirements, and significantly improving the LOI value and mechanical properties at a low addition amount.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878809A_ABST
    Figure CN118878809A_ABST
Patent Text Reader

Abstract

The invention discloses a novel calcium-containing sulfonic acid type ionomer flame retardant as well as a preparation method and application thereof, and belongs to the technical field of flame retardant synthesis. The preparation method of the calcium-containing sulfonic acid type ionomer flame retardant comprises the following steps: mixing polycarbonate and a sulfonation reagent, carrying out sulfonation reaction to obtain sulfonated polycarbonate, mixing the sulfonated polycarbonate with a metal source modified component, and carrying out ion exchange reaction to obtain the calcium-containing sulfonic acid type ionomer flame retardant. The chemical structure of the calcium-containing sulfonic acid type ionomer flame retardant is similar to that of polycarbonate, the synthesis process is simple and easy to operate, after the calcium-containing sulfonic acid type ionomer flame retardant is added into the PC, the influence on the compatibility of a product system is small, the calcium-containing sulfonic acid type ionomer flame retardant is non-toxic, heat-insulating and oxygen-insulating, the high flame-retardant effect can be achieved under the condition of low addition amount, and the high mechanical property of a composite material is kept; popularization and application are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame retardant synthesis, in particular to a novel calcium-containing sulfonic acid type ionomer flame retardant and a preparation method and application thereof. Background Art

[0002] Bisphenol A type PC (polycarbonate) has excellent transparency, high mechanical strength, good stability, high glass transition temperature and electrical insulation performance. It is often selected as a substitute for glass and other types of plastics in many demanding environments. However, the melting drop phenomenon and toxic smoke release of PC during combustion limit its use in some applications with high safety requirements, such as medical equipment, electronic appliances, and automotive parts. These applications usually require that the material not only has self-extinguishing properties, but also does not produce excessive smoke and toxic gases during combustion, and also avoids melting drop phenomenon as much as possible, so as to reduce the risk and harm of fire.

[0003] At present, the commonly used polycarbonate flame retardants can be divided into two categories according to the elements they contain: inorganic flame retardants and organic flame retardants. Inorganic flame retardants and organic flame retardants can be divided into organic / inorganic halogen flame retardants, organic / inorganic phosphorus flame retardants, organic / inorganic boron flame retardants, organic / inorganic silicon flame retardants and organic / inorganic sulfonate flame retardants according to the main elements that play a flame retardant role.

[0004] Among them, sulfonate flame retardants can quickly release a large amount of stable gas at high temperature to form a protective layer, thereby effectively isolating the combustion source and slowing down the spread of fire. They also have good antioxidant properties, can remain stable in high temperature environments, are not prone to decomposition and failure, have good weather resistance in open environments, are not easily affected by ultraviolet rays, moisture and other factors, maintain flame retardant effects for a long time, and can effectively delay the release of smoke generated during combustion. However, the molecular structure of sulfonate flame retardants in the prior art is too different from that of polycarbonate, which easily leads to poor compatibility and thus reduces the mechanical properties of composite materials. For example, the notched impact strength of the composite material of the commercially available KSS sulfonate flame retardant drops to 19.27MPA when the addition amount is 0.2wt.%, which is nearly 70% lower than the 63.35MPa of pure PC material, so further improvement is still needed. Summary of the invention

[0005] The object of the present invention is to provide a novel calcium-containing sulfonic acid type ionomer flame retardant and a preparation method and application thereof, so as to solve the above-mentioned problems in the background technology. The chemical structure of the calcium-containing sulfonic acid type ionomer flame retardant of the present invention is similar to that of polycarbonate, the synthesis process is simple and easy to operate, and the addition of the calcium-containing sulfonic acid type ionomer flame retardant to PC has little effect on the compatibility of the product system, is non-toxic, heat-insulating and oxygen-insulating, can achieve high flame retardant effect at a relatively low addition amount, and maintains the high mechanical properties of the composite material, and is suitable for promotion and application.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] One of the technical solutions of the present invention is to provide a calcium-containing sulfonic acid type ionomer flame retardant, the structural formula of the flame retardant is as follows:

[0008]

[0009] The second technical solution of the present invention is to provide a method for preparing the above-mentioned calcium-containing sulfonic acid type ionomer flame retardant, comprising the following steps:

[0010] The polycarbonate and the sulfonating agent are mixed to carry out a sulfonation reaction to obtain the sulfonated polycarbonate, which is then mixed with the metal source modification component to carry out an ion exchange reaction to obtain the calcium-containing sulfonic acid type ionomer flame retardant.

[0011] Preferably, the sulfonating agent is diethyl sulfate.

[0012] Preferably, the preparation method of diethyl sulfate is: 98wt.% concentrated sulfuric acid and acetic anhydride are mixed in a solvent 1,2-dichloroethane, and an esterification reaction is performed to obtain a solution of intermediate compound II, wherein the intermediate compound II is diethyl sulfate. The relevant reaction formula is shown in formula (I):

[0013]

[0014] More preferably, the temperature of the esterification reaction is 0-5°C, and the volume ratio of concentrated sulfuric acid to acetic anhydride added is 1:2.5.

[0015] Since the reaction between concentrated sulfuric acid and acetic anhydride is violent, the operation needs to be carried out in an ice bath at 0-5°C. After the esterification reaction is completed, it can be observed that the solution system is a yellow oil. When too much acetic anhydride is added, the product solution is colorless and transparent, indicating that the reaction is not complete.

[0016] More preferably, the mass ratio of the polycarbonate to the sulfonated reagent is 1-100:0-10, and is not zero.

[0017] More preferably, the sulfonation reaction is: dissolving polycarbonate in 1,2-dichloroethane, adding diethyl sulfate, and reacting at 60° C. for 2 hours to obtain sulfonated polycarbonate.

[0018] More preferably, the sulfonation reaction is as follows: dissolving polycarbonate in 1,2-dichloroethane, adding diethyl sulfate, reacting at 60°C for 2h, then slowly dropping the reaction system into boiling distilled water, filtering the precipitate, washing and drying, and obtaining a white solid sulfonated polycarbonate (intermediate compound III). The relevant reaction formula is shown in Formula (II):

[0019]

[0020] More preferably, the ratio of 1,2-dichloroethane to polycarbonate is 10 mL:1 g.

[0021] When the reaction temperature exceeds 65°C, the reaction solution becomes dark yellow and the thermal stability of the product decreases.

[0022] During the reaction, the reaction solution was tested with pH test paper, and the reaction was completed when the solution reached neutrality.

[0023] Since the boiling point of 1,2-dichloroethane is 83°C, boiling distilled water is used to remove excess solvent, and then sulfonated polycarbonate is obtained by filtration.

[0024] More preferably, the drying temperature is less than 60°C.

[0025] Preferably, the metal source modifying component is calcium chloride.

[0026] Preferably, the ion exchange reaction is: dissolving the sulfonated polycarbonate in 1,2-dichloroethane, adding calcium chloride, reacting for 48 hours, then slowly dropping the reaction system into boiling distilled water, filtering the precipitate, washing and drying, to obtain the calcium-containing sulfonic acid type ionomer flame retardant (Compound I). The relevant reaction formula is shown in Formula (III):

[0027]

[0028] More preferably, the ratio of 1,2-dichloroethane to sulfonated polycarbonate is 10 mL:1 g.

[0029] More preferably, the drying temperature is less than 60°C.

[0030] More preferably, the added amount of the metal source modification component is 120 wt% of the theoretical required amount; the theoretical required amount is obtained by measuring the sulfonation degree of the sulfonated polycarbonate.

[0031] Preferably, the ion exchange reaction time is 48 hours.

[0032] Preferably, the method for measuring the sulfonation degree of the sulfonated polycarbonate is as follows: dissolving the sulfonated polycarbonate in 1,2-dichloroethane, adding an excess of 0.1 mol / L KOH standard solution, and adding anhydrous ethanol to make the KOH standard solution and the 1,2-dichloroethane solution of the sulfonated polycarbonate completely miscible, and after standing for 30 minutes, adding 0.1 mol / L HCl standard solution dropwise to the solution, and using phenolphthalein as an indicator, taking the color change point as the titration endpoint, and calculating the sulfonation degree of the sulfonated polycarbonate by detecting the volume of the consumed HCl standard solution.

[0033] More preferably, the ratio of the volume of 1,2-dichloroethane to the mass of sulfonated polycarbonate is 5 mL:1 g.

[0034] The third technical solution of the present invention is to provide an application of the above-mentioned calcium-containing sulfonic acid type ionomer flame retardant in the field of polycarbonate flame retardant.

[0035] The fourth technical solution of the present invention is to provide a polycarbonate composite material, wherein the raw materials of the polycarbonate composite material include the above-mentioned calcium-containing sulfonic acid type ionomer flame retardant; the addition amount of the calcium-containing sulfonic acid type ionomer flame retardant is 0-2wt.%, and is not 0.

[0036] The beneficial technical effects of the present invention are as follows:

[0037] The chemical structure of the calcium-containing sulfonic acid ionomer flame retardant of the present invention is similar to that of polycarbonate, the synthesis process is simple and easy to operate, and the addition of the calcium-containing sulfonic acid ionomer flame retardant to PC has little effect on the compatibility of the product system, is non-toxic, heat-insulating and oxygen-insulating, can achieve a high flame retardant effect at a relatively low addition amount, and maintains high mechanical properties of the composite material, and is suitable for popularization and application. When 2wt.% of the flame retardant with a sulfonation degree of 5wt.% is added, the LOI value of the composite material is 36%, and passes the UL-94V-0 grade.

[0038] The flame retardant system designed by the present invention improves the flame retardancy of the polycarbonate composite material while also improving mechanical properties such as impact strength and flexural strength to a certain extent. The calcium-containing sulfonic acid-type ionomer flame retardant designed by the present invention has little effect on the mechanical properties and transparency of polycarbonate after addition. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0040] Figure 1 The present invention is a flow chart of the preparation method of Examples 1-3.

[0041] Figure 2 This is the Fourier transform infrared spectrum of the product of Example 3 of the present invention. DETAILED DESCRIPTION

[0042] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0043] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0044] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.

[0045] The words “include,” “including,” “have,” “contain,” etc. used in the present invention are open-ended terms, meaning including but not limited to.

[0046] The present invention provides a method for preparing a calcium-containing sulfonic acid type ionomer flame retardant, comprising the following steps:

[0047] The polycarbonate and the sulfonating agent are mixed to carry out a sulfonation reaction to obtain the sulfonated polycarbonate, which is then mixed with the metal source modification component to carry out an ion exchange reaction to obtain the calcium-containing sulfonic acid type ionomer flame retardant.

[0048] Preferably, the preparation method of diethyl sulfate is: mixing 98wt.% concentrated sulfuric acid with acetic anhydride, and performing an esterification reaction to obtain a solution of intermediate compound II, wherein the intermediate compound II is diethyl sulfate. The relevant reaction formula is shown in formula (I):

[0049]

[0050]

[0051] More preferably, the temperature of the esterification reaction is 0-5°C, and the volume ratio of concentrated sulfuric acid to acetic anhydride added is 1:2.5.

[0052] Since the reaction between concentrated sulfuric acid and acetic anhydride is violent, the operation needs to be carried out in an ice bath at 0-5°C. After the esterification reaction is completed, it can be observed that the solution system is a yellow oil. When too much acetic anhydride is added, the product solution is colorless and transparent, indicating that the reaction is not complete.

[0053] More preferably, the sulfonation reaction is as follows: dissolving polycarbonate in 1,2-dichloroethane, adding diethyl sulfate, reacting at 60°C for 2h, then slowly dropping the reaction system into boiling distilled water, filtering the precipitate, washing and drying, and obtaining a white solid sulfonated polycarbonate (intermediate compound III). The relevant reaction formula is shown in Formula (II):

[0054]

[0055] More preferably, the ratio of 1,2-dichloroethane to polycarbonate is 10 mL:1 g.

[0056] When the reaction temperature exceeds 65°C, the reaction solution becomes dark yellow and the thermal stability of the product decreases.

[0057] During the reaction, the reaction solution was tested with pH test paper, and the reaction was completed when the solution reached neutrality.

[0058] Since the boiling point of 1,2-dichloroethane is 83°C, boiling distilled water is used to remove excess solvent, and then sulfonated polycarbonate is obtained by filtration.

[0059] More preferably, the drying temperature is less than 60°C.

[0060] Preferably, the method for measuring the sulfonation degree of the sulfonated polycarbonate is as follows: dissolving the sulfonated polycarbonate in 1,2-dichloroethane, adding an excess of 0.1 mol / L KOH standard solution, and adding anhydrous ethanol to make the KOH standard solution and the 1,2-dichloroethane solution of the sulfonated polycarbonate completely miscible, and after standing for 30 minutes, adding 0.1 mol / L HCl standard solution dropwise to the solution, and using phenolphthalein as an indicator, taking the color change point as the titration endpoint, and calculating the sulfonation degree of the sulfonated polycarbonate by detecting the volume of the consumed HCl standard solution.

[0061] More preferably, the ratio of 1,2-dichloroethane to sulfonated polycarbonate is 5 mL:1 g.

[0062] Preferably, the ion exchange reaction is: dissolving the sulfonated polycarbonate in 1,2-dichloroethane, adding calcium chloride, reacting for 48 hours, then slowly dropping the reaction system into boiling distilled water, filtering the precipitate, washing and drying, to obtain the calcium-containing sulfonic acid type ionomer flame retardant (Compound I). The relevant reaction formula is shown in Formula (III):

[0063]

[0064] More preferably, the ratio of 1,2-dichloroethane to sulfonated polycarbonate is 10 mL:1 g.

[0065] More preferably, the drying temperature is less than 60°C.

[0066] The method for measuring the sulfonation degree of the sulfonated polycarbonate in the following embodiments of the present invention is as follows: dissolving the sulfonated polycarbonate in 1,2-dichloroethane (the ratio of 1,2-dichloroethane to the sulfonated polycarbonate is 5 mL: 1 g), adding an excess of 0.1 mol / L KOH standard solution, and adding anhydrous ethanol to make the KOH standard solution and the 1,2-dichloroethane solution of the sulfonated polycarbonate completely miscible, and after standing for 30 minutes, adding 0.1 mol / L HCl standard solution dropwise to the solution, and using phenolphthalein as an indicator, taking the color change point as the titration end point, and calculating the sulfonation degree of the sulfonated polycarbonate by detecting the volume of the consumed HCl standard solution.

[0067] The concentration of concentrated sulfuric acid used in the following examples of the present invention is 98wt.%.

[0068] The temperature of the boiling distilled water used in the following embodiments of the present invention is 100°C.

[0069] All raw materials used in the following embodiments of the present invention are commercially available products.

[0070] Example 1

[0071] A preparation method of a calcium-containing sulfonic acid-type ionomer flame retardant:

[0072] First, 1 mL of concentrated sulfuric acid and 2.5 mL of acetic anhydride were dissolved in 1,2-dichloroethane, and esterification reaction was carried out at 0°C to obtain diethyl sulfate. 100 g of polycarbonate was dissolved in 1 L of 1,2-dichloroethane, and diethyl sulfate obtained in the first step was added under stirring at 60°C for 2 hours, and then the reaction system was slowly added dropwise to boiling distilled water, the precipitate was filtered, washed and dried (drying temperature < 60°C), and a white solid sulfonated polycarbonate was obtained (the sulfonation degree of the sulfonated polycarbonate was 1 wt.%).

[0073] 10 g of sulfonated polycarbonate was dissolved in 100 mL of 1,2-dichloroethane, 0.15 g of calcium chloride (20 wt% excess) was added to distilled water to dissolve, and then poured into the solution system, stirred for 48 hours for ion exchange reaction, and then the reaction system was slowly added dropwise to boiling distilled water, the precipitate was filtered, washed and dried (drying temperature <60°C), and a calcium-containing sulfonic acid type ionomer flame retardant (denoted as SPC-Ca) was obtained.

[0074] Example 2

[0075] A preparation method of a calcium-containing sulfonic acid-type ionomer flame retardant:

[0076] First, 2 mL of concentrated sulfuric acid and 5 mL of acetic anhydride were dissolved in 1,2-dichloroethane, and esterification reaction was carried out at 0°C to obtain diethyl sulfate. 100 g of polycarbonate was dissolved in 1 L of 1,2-dichloroethane, and diethyl sulfate obtained in the first step was added under stirring at 60°C for 2 h, and then the reaction system was slowly added dropwise to boiling distilled water, the precipitate was filtered, washed and dried (drying temperature < 60°C), and a white solid sulfonated polycarbonate was obtained (the sulfonation degree of the sulfonated polycarbonate was 3 wt.%).

[0077] 5 g of sulfonated polycarbonate was dissolved in 50 mL of 1,2-dichloroethane, 0.24 g of calcium chloride was added to distilled water and dissolved, and then poured into the solution system, stirred for 48 hours for ion exchange reaction, and then the reaction system was slowly added dropwise to boiling distilled water, the precipitate was filtered, washed and dried (drying temperature <60°C), and a calcium-containing sulfonic acid type ionomer flame retardant (denoted as SPC-Ca) was obtained.

[0078] Example 3

[0079] A preparation method of a calcium-containing sulfonic acid-type ionomer flame retardant:

[0080] First, 5 mL of concentrated sulfuric acid and 12.5 mL of acetic anhydride were dissolved in 1,2-dichloroethane, and esterification reaction was carried out at 0°C to obtain diethyl sulfate. 100 g of polycarbonate was dissolved in 1 L of 1,2-dichloroethane, and diethyl sulfate obtained in the first step was added under stirring at 60°C for 2 hours, and then the reaction system was slowly added dropwise to boiling distilled water, the precipitate was filtered, washed and dried (drying temperature < 60°C), and a white solid sulfonated polycarbonate was obtained (the sulfonation degree of the sulfonated polycarbonate was 1 wt.%).

[0081] 20 g of sulfonated polycarbonate was dissolved in 200 mL of 1,2-dichloroethane, 5 g of calcium chloride was added to distilled water and dissolved, and then poured into the solution system, stirred for 48 hours for ion exchange reaction, and then the reaction system was slowly added dropwise to boiling distilled water, the precipitate was filtered, washed and dried (drying temperature <60°C), and a calcium-containing sulfonic acid type ionomer flame retardant (denoted as SPC-Ca) was obtained.

[0082] Figure 1 The present invention is a flow chart of the preparation method of Examples 1-3.

[0083] Figure 2 This is the Fourier transform infrared spectrum of the product of Example 3 of the present invention.

[0084] Figure 2 Medium, 3455cm -1Nearby is the OH stretching vibration peak. Since there is no OH stretching vibration peak in the infrared characteristic peak of polycarbonate, it can be proved that it comes from the sulfonic acid group introduced by the sulfonation reaction; 2919cm -1 The peak near 1619cm is the CH stretching vibration peak, which comes from the isopropylidene group in the sulfonated polycarbonate, proving that it does not break during the sulfonation reaction; -1 The C=O stretching vibration absorption peak is at 1285cm, which proves that the two bonds with the smallest dissociation energy are not destroyed in the sulfonation reaction. -1 The absorption peak between is caused by the stretching vibration of the sulfonic acid group S=O. The sulfonated product is at 1072 cm -1 The stretching vibration absorption peak of the sulfonic acid group on the benzene ring is difficult to distinguish at 769cm -1 Nearby, an absorption peak representing the in-plane bending vibration of the sulfonic acid group-substituted benzene ring appears.

[0085] Effect verification

[0086] The polycarbonate composite material was prepared as follows:

[0087] (1) The PC masterbatch was placed in a 100°C forced air drying oven and dried for 10 hours, and then the products of each embodiment and the commercial KSS flame retardant were mixed with the PC masterbatch in different proportions, and then extruded, cooled, and granulated by a twin-screw extruder to obtain pellets; during this period, the screw speed was 100 r / min. The temperature of each temperature section set by the twin-screw extruder is shown in Table 1.

[0088] Table 1 Temperature of each temperature section of twin screw extruder

[0089]

[0090] (2) The pellets were placed in a 100°C forced air drying oven and dried for 10 h. Then, in accordance with GB / T 25156-2010, an experimental standard specimen (polycarbonate composite material) was obtained using an injection molding machine. The LOI value (limiting oxygen index) of the experimental standard specimen was obtained using the ISO4589-1996 standard test, and the specimen specification was 120 mm × 10 mm × 4 mm. The vertical combustion test was measured using the UL-94 standard, and the specimen specification was 120 mm × 13 mm × 3.2 mm. Injection molding pressure: 50 MPa for the first and second sections, respectively. The temperatures of each temperature section of the injection molding machine are shown in Table 2. The limiting oxygen index and vertical combustion test results are shown in Table 3. The mechanical properties test results are shown in Table 4.

[0091] Table 2 Temperature of each temperature range of injection molding machine

[0092]

[0093] Table 3 Flame retardant performance test at different flame retardant addition amounts

[0094]

[0095] As can be seen from Table 3, the LOI value of the experimental standard specimen prepared from pure PC is 26.8%, and the UL-94 vertical combustion grade is UL-94V-2. As the amount of flame retardant added increases, the LOI value of the composite material gradually increases. When 1wt.% of a flame retardant with a sulfonation degree of 1wt.% is added, the LOI value of the composite material is 33.5%, and it passes the UL-94V-0 grade; when 2wt.% of a flame retardant with a sulfonation degree of 5wt.% is added, the LOI value of the composite material is 36.5%, and it passes the UL-94V-0 grade. This shows that the calcium-containing sulfonic acid type ionomer flame retardant prepared by the present invention can well improve the LOI value of the composite material, showing a good flame retardant effect, and is ahead of the commercial KSS flame retardant.

[0096] In summary, calcium-containing sulfonic acid-based ionomer flame retardants play an effective flame retardant role and improve the flame retardant properties of the substrate. This may be because it can decompose and rearrange PC in advance, and cause cross-linking reactions, increase the stability and density of the carbon layer, and play a role in isolating oxygen.

[0097] Table 4 Mechanical properties test of SPC-Ca at different addition amounts

[0098]

[0099]

[0100] As shown in Table 4, the composite material to which the novel calcium-containing sulfonic acid-type ionomer flame retardant of the present invention is added has enhanced flexural strength and elongation at break while maintaining the same tensile strength and slightly reducing the notched impact strength.

[0101] The flame retardant designed in the present invention has a novel structure, is non-toxic, is heat-insulating and oxygen-insulating, achieves a high flame retardant effect at a low addition amount, and does not affect the mechanical properties. At the same time, the synthesis process is simple, easy to operate, and suitable for popularization and application.

[0102] The embodiments described above are only descriptions of the preferred embodiments of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A calcium-containing sulfonic acid type ionomer flame retardant, characterized in that: The structural formula of the flame retardant is as follows:

2. A method for preparing the calcium-containing sulfonic acid type ionomer flame retardant according to claim 1, characterized in that: The following steps are involved: The polycarbonate and the sulfonating agent are mixed to carry out a sulfonation reaction to obtain the sulfonated polycarbonate, which is then mixed with the metal source modification component to carry out an ion exchange reaction to obtain the calcium-containing sulfonic acid type ionomer flame retardant.

3. The preparation method according to claim 2, characterized in that: The sulfonating agent is diethyl sulfate.

4. The preparation method according to claim 3, characterized in that: The sulfonation reaction is as follows: polycarbonate is dissolved in 1,2-dichloroethane, diethyl sulfate is added, and the reaction is carried out at 60° C. for 1-5 hours to obtain sulfonated polycarbonate.

5. The preparation method according to claim 3, characterized in that: The mass ratio of the polycarbonate to the sulfonated reagent is 1-100:0-10, and is not zero.

6. The preparation method according to claim 2, characterized in that: The metal source modification component is calcium chloride.

7. The preparation method according to claim 6, characterized in that: The added amount of the metal source modification component is 120 wt% of the theoretical required amount; the theoretical required amount is obtained by measuring the sulfonation degree of the sulfonated polycarbonate.

8. The preparation method according to claim 2, characterized in that: The ion exchange reaction time is 48h.

9. Use of the calcium-containing sulfonic acid type ionomer flame retardant according to claim 1 in the field of polycarbonate flame retardants.

10. A polycarbonate composite material, characterized in that: The raw materials of the polycarbonate composite material include the calcium-containing sulfonic acid type ionomer flame retardant according to claim 1; the addition amount of the calcium-containing sulfonic acid type ionomer flame retardant is 0-2wt.%, and is not 0.

Citation Information

Patent Citations

  • Novel magnesium-containing sulfonate type flame retardant as well as preparation method and application thereof

    CN116751144A

  • Flame retardant, flame-retarded resin compositions, and process for production of the flame retardant

    WO2005090468A1

  • High-toughness and high-fluidity flame-retardant polycarbonate composition, preparation method therefor, and application thereof

    WO2022083062A1

  • Thermoplastic ABS moulding compound with a good property combination of processability and surface quality

    WO2024028309A1

Cited By

  • Polysiloxane-based flame retardant, preparation method thereof and polycarbonate composite flame-retardant material

    CN121181899A

  • A polysiloxane-based flame retardant, a method for preparing the same, and a polycarbonate composite flame retardant material

    CN121181899B