Solid-state battery and preparation method thereof
By integrating multi-nozzle 3D printing and lamination of solid-state battery cells, the problem of balancing solid-state battery production efficiency and battery performance in the existing technology is solved, achieving efficient manufacturing and improving battery cell performance.
Patent Information
- Application Number
- CN202411080037.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-10-29
AI Technical Summary
In the existing technology, when 3D printing is used to prepare solid-state batteries, it is difficult to balance production efficiency and battery performance. Printing the positive electrode, negative electrode and solid electrolyte separately leads to high internal resistance and reduced rate performance.
Multi-nozzle integrated 3D printing is used to 3D print the entire solid-state battery core, including the bipolar current collector layer, positive electrode layer, solid electrolyte layer and negative electrode layer, which are printed sequentially from bottom to top and laminated. After printing, the battery unit is laminated. Pressure greater than 100 MPa, combined with binder jet printing and selective laser sintering processes.
The manufacturing efficiency and output voltage are significantly improved, the energy density of the battery core is enhanced, the grain gap is reduced, and the ion transmission capability is improved.
Smart Images

Figure CN118867413A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid-state batteries, and in particular to a solid-state battery and a preparation method thereof. Background Art
[0002] All-solid-state batteries refer to the use of solid electrolytes to replace the electrolyte and separator of traditional lithium-ion batteries, while matching high-capacity positive and negative electrodes to intrinsically improve the safety and energy density of the battery. The emerging 3D printing technology can customize complex three-dimensional structures of electrodes and solid electrolyte structures according to demand, which can improve the performance of solid-state batteries.
[0003] However, the current 3D printing technology for preparing lithium-ion batteries is relatively complicated. Usually, the positive and negative electrodes are printed separately and then assembled into batteries with solid electrolytes in a glove box. The process is cumbersome and time-consuming, and cannot fully utilize the advantages of 3D printing.
[0004] In the prior art, patent application CN 114865096 A combines the advantages of ink direct writing and photocuring technology, realizes the layer-by-layer molding of positive electrode, negative electrode and solid electrolyte by photocuring, simplifies the molding ink formula and printing process, and is conducive to process scale. However, it obtains a single-layer solid-state battery component, does not indicate whether a multi-layer solid-state battery can be prepared, and is printed by a single nozzle, with low printing efficiency. At the same time, there is no subsequent lamination and current collector accessories, which will lead to a large internal resistance after the battery is connected in series, resulting in reduced rate performance. Patent application CN 115224369 A designs convex and concave features at the interface between the electrode and the solid electrolyte to increase the interface contact area. The positive electrode slurry is coated at the interface between the positive electrode and the solid electrolyte to improve the wettability of the interface. The positive electrode and solid electrolyte are formed by indirect 3D printing process to achieve batch manufacturing; the positive electrode and electrolyte are densified by sintering to improve the ionic conductivity. However, it still prints the positive and negative electrodes and the solid electrolyte separately, and then assembles them, which reduces production efficiency.
[0005] Therefore, although the prior art has disclosed the use of 3D printing methods to prepare solid-state batteries, existing applications cannot well balance production efficiency and battery performance, and there is still room for further improvement. Summary of the invention
[0006] The present invention provides a solid-state battery and a preparation method thereof, so as to solve the defect that the production efficiency and battery performance cannot be taken into account when the solid-state battery is prepared by the 3D printing method in the prior art, and give full play to the advantages of 3D printing.
[0007] In a first aspect, the present invention provides a method for preparing a solid-state battery, comprising: using 3D printing to print the entire solid-state battery cell in an integrated manner to obtain a solid-state battery cell block; and then laminating the solid-state battery cell block; wherein the solid-state battery cell block includes, from bottom to top, a bipolar current collector layer, a positive electrode layer, a solid electrolyte layer, a negative electrode layer and a bipolar current collector layer.
[0008] According to a method for preparing a solid-state battery provided by the present invention, when 3D printing a solid-state battery, each 3D printing nozzle corresponds to one raw material, and multiple layers are printed simultaneously.
[0009] According to a method for preparing a solid-state battery provided by the present invention, when performing 3D printing, from bottom to top, the bipolar current collector layer is printed first, and the positive electrode layer is printed on the bipolar current collector layer 0.5 to 2 minutes later; then the solid electrolyte layer is printed on the positive electrode layer 0.5 to 2 minutes later, and then the negative electrode layer is printed on the solid electrolyte layer 0.5 to 2 minutes later, and then the bipolar current collector is printed on the negative electrode layer 0.5 to 2 minutes later, to achieve simultaneous printing of multiple layers, and after the printing is completed, it is a battery unit.
[0010] According to a method for preparing a solid-state battery provided by the present invention, the lamination includes a roller pressing or isostatic pressing process, and the lamination pressure is greater than 100 MPa.
[0011] According to a method for preparing a solid-state battery provided by the present invention, during the 3D printing process, single-layer rolling is performed while printing each layer; preferably, the pressure of the single-layer rolling is 5-15 MPa.
[0012] According to a method for preparing a solid-state battery provided by the present invention, the 3D printing process includes one or more of a binder jet printing process, a fused deposition printing process and a selective laser sintering printing process.
[0013] According to a method for preparing a solid-state battery provided by the present invention, the positive electrode layer and the negative electrode layer are printed using the binder jetting process.
[0014] According to a method for preparing a solid-state battery provided by the present invention, the raw material of the bipolar current collector layer includes stainless steel foil and / or aluminum-copper composite foil.
[0015] According to a method for preparing a solid-state battery provided by the present invention, the raw materials of the positive electrode layer include a positive electrode active material, a conductive agent, a binder and a solid electrolyte; preferably, the positive electrode active material includes lithium iron phosphate, lithium cobalt oxide, lithium nickel manganese oxide, ternary nickel cobalt manganese oxide or lithium-rich manganese base; the conductive agent includes one or more of super-p, conductive carbon black, acetylene black, graphene and carbon nanotubes; the binder includes polytetrafluoroethylene, polyvinyl pyrrolidone and / or polyvinylidene fluoride.
[0016] According to a method for preparing a solid-state battery provided by the present invention, the raw materials of the solid electrolyte layer include one or more of an oxide solid electrolyte, a sulfide solid electrolyte and a halide solid electrolyte; preferably, the oxide solid electrolyte includes one or more of lithium lanthanum zirconium oxide with a garnet structure, lithium lanthanum zirconium tantalum oxide with a garnet structure, lithium aluminum titanium phosphate with a NASICON structure and lithium aluminum germanium phosphate with a NASICON structure; the sulfide solid electrolyte includes one or more of lithium phosphorus sulfur chlorine, lithium germanium phosphorus sulfur, lithium tin phosphorus sulfur, lithium phosphorus sulfur and lithium tin sulfur; the halide solid electrolyte includes one or more of lithium indium chloride, lithium holmium chloride, lithium yttrium chloride, lithium scandium chloride and lithium erbium chloride.
[0017] According to a method for preparing a solid-state battery provided by the present invention, the raw material of the negative electrode includes one or more of graphite, silicon carbon, metallic lithium and lithium alloy.
[0018] According to a method for preparing a solid-state battery provided by the present invention, when the raw material of the solid electrolyte layer is an oxide solid electrolyte, sintering is further performed after the lamination, and the sintering temperature is 200~1100 degrees Celsius; and other solid electrolytes except the oxide solid electrolyte are not sintered after the lamination.
[0019] A method for preparing a solid-state battery provided by the present invention comprises: S1: prepare bipolar current collector powder, positive electrode powder, negative electrode powder and solid electrolyte printing powder; S2: printing the entire solid-state battery cell in an integrated manner to obtain a solid-state battery cell block; during the 3D printing process, single-layer rolling is performed while printing each layer; S3: laminating the solid-state battery cell blocks; S4: Cut the laminated solid battery cell blocks according to the battery cell size requirements; S5: Encapsulating the cut battery cells to obtain solid-state battery cells connected in series; When the raw material of the solid electrolyte layer is an oxide solid electrolyte, the cutting further includes sintering, and the sintering temperature is 200-1100 degrees Celsius.
[0020] In a second aspect, the present invention provides a solid-state battery, which is prepared by the solid-state battery preparation method.
[0021] The solid-state battery and preparation method thereof provided by the present invention directly obtain solid-state battery cells by adopting multi-nozzle integrated printing, which can not only greatly improve the manufacturing efficiency and realize batch manufacturing; but also the bipolar current collector can realize the internal series connection of the solid-state battery, increase the output voltage, and further increase the energy density of the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 It is a schematic diagram of the solid-state battery unit structure provided in Example 1 of the present invention.
[0024] Figure 2 This is a schematic diagram of a 3D printed solid-state battery provided in Example 1 of the present invention.
[0025] Figure 3 This is a process flow chart of 3D printing solid-state batteries provided in Example 3 of the present invention. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] At present, although the existing technology has disclosed the use of 3D printing methods to prepare solid-state batteries, existing applications cannot well balance production efficiency and battery performance, that is, there is still room for further improvement when using 3D printing methods to prepare solid-state batteries.
[0028] The present invention found that the main reason for the above problems is that the existing technology uses a single nozzle printing method to prepare solid-state batteries using 3D printing, and the positive electrode, negative electrode, and solid electrolyte are formed layer by layer (such as patent application CN 114865096A); patent application CN 115224369 A also prints the positive and negative electrodes and solid electrolyte separately, and then assembles them, which greatly reduces production efficiency. Most importantly, the lack of subsequent lamination and current collector accessories will lead to a large internal resistance after the battery is connected in series, resulting in reduced rate performance.
[0029] In this regard, the present invention first discovered and proposed the integrated 3D printing of the negative electrode layer, solid electrolyte layer, positive electrode layer and bipolar current collector layer by multiple nozzles, which does not require further assembly and can significantly improve production efficiency; at the same time, combined with the lamination after printing, it can significantly improve the output voltage and energy density.
[0030] Based on this, the present invention has the following technical solutions: In a first aspect, the present invention provides a method for preparing a solid-state battery, comprising: using 3D printing to print the entire solid-state battery cell in an integrated manner to obtain a solid-state battery cell block; and then laminating the solid-state battery cell block; wherein the solid-state battery cell block includes, from bottom to top, a bipolar current collector layer, a positive electrode layer, a solid electrolyte layer, a negative electrode layer and a bipolar current collector layer.
[0031] In the present invention, by adopting 3D printing to print the entire solid-state battery cell in an integrated manner, the advantages of 3D printing can be effectively utilized, while improving the production efficiency and battery performance of the solid-state battery.
[0032] In particular, unlike the existing solid-state batteries which are directly 3D printed on the solid current collector plate of the finished product, the current collector is customized and printed in an integrated manner. The integrated printing process increases the composite effect of the electrode material and the current collector, thereby enhancing the performance of the battery cell.
[0033] In the present invention, when the current collector is 3D printed, the structure of the current collector can be customized and designed. For example, for the negative electrode lithium metal, the three-dimensional structure is similar to the porous structure of sponge, which can also alleviate the volume change problem caused by lithium deposition during the subsequent battery charging and discharging process.
[0034] According to a preferred embodiment provided by the present invention, when 3D printing a solid-state battery, each 3D printing nozzle corresponds to one raw material, and multiple layers are printed simultaneously.
[0035] In the present invention, printing multiple layers simultaneously does not mean that multiple layers start printing at the same time, but that the bipolar current collector layer is printed first from bottom to top, and the positive electrode layer is printed after waiting for 0.5 to 2 minutes, at which time the bipolar current collector layer is still being printed; and so on, the solid electrolyte layer, the negative electrode layer and the bipolar current collector layer are printed in sequence until the top bipolar current collector layer is printed, that is, a battery unit is completed.
[0036] In the present invention, according to the performance requirements of the solid-state battery, multiple 3D printing nozzles are provided to print multiple battery cells simultaneously, which not only omits the subsequent further assembly but also further improves the battery performance.
[0037] According to a method for preparing a solid-state battery provided by the present invention, when performing 3D printing, from bottom to top, the bipolar current collector layer is printed first, and the positive electrode layer is printed on the bipolar current collector layer 0.5 to 2 minutes later; then the solid electrolyte layer is printed on the positive electrode layer 0.5 to 2 minutes later, and then the negative electrode layer is printed on the solid electrolyte layer 0.5 to 2 minutes later, and then the bipolar current collector is printed on the negative electrode layer 0.5 to 2 minutes later, to achieve simultaneous printing of multiple layers, and after the printing is completed, it is a battery unit.
[0038] According to a preferred embodiment provided by the present invention, the lamination includes a roller pressing or isostatic pressing process, and the lamination pressure is greater than 100 MPa.
[0039] Further preferably, the lamination pressure is 100-500 MPa, specifically 100 MPa, 150 MPa, 200 MPa, 250 MPa, 300 MPa, 350 MPa, 400 MPa, 450 MPa or 500 MPa.
[0040] In the present invention, by controlling the lamination pressure within the above range, the density of the electrode and the solid electrolyte layer can be greatly improved, the grain gap can be reduced, and the ion transmission capacity of the battery cell can be improved; when the lamination pressure is lower than 100 MPa, the grain gap may be too large, thereby reducing the ion transmission capacity of the battery cell.
[0041] According to a preferred embodiment provided by the present invention, during the 3D printing process, single-layer rolling is performed while printing each layer; more preferably, the pressure of the single-layer rolling is 5-15 MPa.
[0042] In the present invention, the thickness of the bipolar current collector layer is 5 to 20 microns; the thickness of the positive electrode layer can be adjusted according to demand, preferably 100 to 500 microns; the thickness of the solid electrolyte layer is 5 to 30 microns; the thickness of the negative electrode layer is determined according to the positive electrode capacity; specifically, the thickness of the silicon-carbon negative electrode is 70 to 400 microns, and the thickness of the lithium metal is 20 to 100 microns.
[0043] According to a preferred embodiment provided by the present invention, the 3D printing process includes one or more of a binder jet printing process, a fused deposition printing process and a selective laser sintering printing process. Those skilled in the art may use the above-mentioned process technologies disclosed in the prior art to perform 3D printing, and the specific process technology scheme is not limited herein.
[0044] According to a preferred embodiment provided by the present invention, the positive electrode layer and the negative electrode layer are printed by the binder jetting process.
[0045] In the present invention, the binder jet printing process used for the positive and negative electrodes can be well adapted to different positive and negative electrode materials, different printing shapes can be set according to requirements, and dry electrode manufacturing can be achieved.
[0046] According to a preferred embodiment provided by the present invention, the raw material of the bipolar current collector layer includes stainless steel foil and / or aluminum-copper composite foil.
[0047] According to a preferred embodiment provided by the present invention, the raw materials of the positive electrode layer include positive electrode active material, conductive agent, binder and solid electrolyte.
[0048] More preferably, the positive electrode active material includes lithium iron phosphate, lithium cobalt oxide, lithium nickel manganese oxide, ternary nickel cobalt manganese oxide or lithium-rich manganese base; the conductive agent includes one or more of super-p, conductive carbon black, acetylene black, graphene and carbon nanotubes; the binder includes polytetrafluoroethylene, polyvinyl pyrrolidone (PVP) and / or polyvinylidene fluoride (PVDF).
[0049] Further preferably, the raw materials of the positive electrode layer include 65-85 parts by weight of positive electrode active material, 1-5 parts by weight of conductive agent, 1-5 parts by weight of binder and 10-25 parts by weight of solid electrolyte.
[0050] According to a preferred embodiment provided by the present invention, the raw material of the solid electrolyte layer includes one or more of an oxide solid electrolyte, a sulfide solid electrolyte and a halide solid electrolyte.
[0051] More preferably, the oxide solid electrolyte includes one or more of lithium lanthanum zirconium oxide (LLZO) with a garnet structure, lithium lanthanum zirconium tantalum oxide (LLZTO) with a garnet structure, lithium aluminum titanium phosphate (LATP) with a NASICON structure, and lithium aluminum germanium phosphate (LAGP) with a NASICON structure; the sulfide solid electrolyte includes one or more of lithium phosphorus sulfur chloride (LPSC), lithium germanium phosphorus sulfur (LGPS), lithium tin phosphorus sulfur (LSPS), lithium phosphorus sulfur (LPS), and lithium tin sulfur (LSP); the halide solid electrolyte includes one or more of lithium indium chloride (LIC), lithium holmium chloride (LHC), lithium yttrium chloride (LYC), lithium scandium chloride (LSC), and lithium erbium chloride (LEC).
[0052] In the present invention, the solid electrolyte in the positive electrode layer raw material and the solid electrolyte in the solid electrolyte layer can be selected from the above list in the same or different manner depending on the selection of the positive electrode active material.
[0053] According to a preferred embodiment provided by the present invention, the raw material of the negative electrode includes one or more of graphite, silicon carbon, metallic lithium and lithium alloy. More preferably, the raw material of the negative electrode is metallic lithium and / or lithium alloy.
[0054] According to a preferred embodiment provided by the present invention, when the raw material of the solid electrolyte layer is an oxide solid electrolyte, sintering is further performed after the lamination, and the sintering temperature is 200~1100 degrees Celsius; and other solid electrolytes except the oxide solid electrolyte are not sintered after the lamination.
[0055] More preferably, the sintering time is 5 to 20 hours.
[0056] In the present invention, only when the raw material of the solid electrolyte layer is an oxide solid electrolyte, the lamination further includes sintering, which can make the positive electrode and the solid electrolyte layer more compact on the one hand, and make the positive and negative electrodes in closer contact with the solid electrolyte layer on the other hand, thereby improving ion conductivity, reducing the internal impedance of the battery, and improving the rate performance and energy density of the battery cell; other solid electrolytes can be directly cut and packaged after lamination.
[0057] A preferred embodiment provided according to the present invention includes: S1: prepare bipolar current collector powder, positive electrode powder, negative electrode powder and solid electrolyte printing powder; S2: printing the entire solid-state battery cell in an integrated manner to obtain a solid-state battery cell block; during the 3D printing process, single-layer rolling is performed while printing each layer; S3: laminating the solid-state battery cell blocks; S4: Cut the laminated solid battery cell blocks according to the battery cell size requirements; S5: Encapsulating the cut battery cells to obtain solid-state battery cells connected in series; When the raw material of the solid electrolyte layer is an oxide solid electrolyte, sintering is further performed after the cutting, and the sintering temperature is 200-1100 degrees Celsius; and other solid electrolytes except the oxide solid electrolyte are not sintered after the lamination.
[0058] In the present invention, the cutting refers to cutting the large battery cell horizontally and vertically to make it into completely separated independent battery cells. The production efficiency can be further improved by first manufacturing large-area battery cells and then cutting them according to needs.
[0059] In a second aspect, the present invention provides a solid-state battery, which is prepared by the solid-state battery preparation method.
[0060] In order to further illustrate the technical solution of the present invention, the present invention provides the following specific embodiments and comparative examples.
[0061] Unless otherwise specified, the various raw materials used in the examples and comparative examples are commercially available conventional raw materials, and the technical means used are conventional means well known to those skilled in the art.
[0062] In the following embodiments, the thickness of the bipolar current collector layer is 10 microns, the thickness of the positive electrode layer is 200 microns, and the thickness of the solid electrolyte layer is 10 microns; when the negative electrode is a silicon-carbon negative electrode, the thickness of the negative electrode is 130 microns, and when the negative electrode is a negative electrode, the thickness of the negative electrode is 60 microns.
[0063] Example 1
[0064] This embodiment provides a solid-state battery, and the preparation method thereof includes: 1. Prepare stainless steel current collector powder, lithium iron phosphate positive electrode powder (including 70 parts of lithium iron phosphate powder, 2 parts of conductive carbon black, 2 parts of polytetrafluoroethylene, 26 parts of lithium titanium aluminum phosphate solid electrolyte), silicon carbon negative electrode powder (including 80 parts of silicon carbon powder, 1 part of conductive carbon black, 4 parts of polyvinyl pyrrolidone, 15 parts of lithium phosphorus sulfur chlorine solid electrolyte) and lithium phosphorus sulfur chlorine solid electrolyte powder for use; 2. Set up 13 3D printing nozzles to prepare 3 layers of solid-state battery cell blocks: nozzle 1 uses selective laser sintering technology to print bipolar current collectors. After 1 to 2 minutes, nozzle 2 uses binder injection molding technology to print lithium iron phosphate powder on the current collector. After 1 to 2 minutes, nozzle 3 uses selective laser sintering technology to print solid electrolyte powder on the positive electrode layer. After 1 to 2 minutes, nozzle 4 uses binder injection molding technology to print silicon carbon powder on the solid electrolyte layer. Repeat the above preparation unit to print 13 layers in total, from bottom to top, in order: bipolar current collector layer, positive electrode layer, solid electrolyte layer, negative electrode layer, bipolar current collector layer, positive electrode layer, solid electrolyte layer, negative electrode layer, bipolar current collector layer, positive electrode layer, solid electrolyte layer, negative electrode layer and bipolar current collector layer, and finally obtain solid-state battery cell blocks; when printing layer by layer, each layer is printed with a roller, and roller pressing is performed immediately after printing. The rolling pressure of a single layer is 10 MPa.
[0065] 3. The obtained solid-state battery cell block is subjected to isostatic pressing at a pressure of 300 MPa, a temperature of 25 degrees Celsius, and a time of 10 minutes; 4. Cut the block to obtain a solid-state battery cell with a size of 4 cm × 4 cm; 5. Weld the pole ears on both sides of the solid-state battery cell and encapsulate it with an aluminum-plastic film to obtain a finished battery cell.
[0066] Figure 1 Schematic diagram of the solid-state battery cell structure provided in this embodiment. Figure 2 is a schematic diagram of a 3D printed solid-state battery provided in this embodiment. It should be noted that: Figure 1~Figure 2 The figure does not show the complete printing of all solid-state batteries, but is just a schematic diagram of the process of printing to the first battery cell.
[0067] Example 2
[0068] This embodiment provides a solid-state battery, and the preparation method thereof includes: 1. Prepare stainless steel current collector powder, ternary positive electrode powder (including 80 parts of NCM811, 2 parts of super-p, 3 parts of polyvinylidene fluoride, 15 parts of lithium lanthanum zirconium oxygen solid electrolyte), lithium / indium metal powder and lithium phosphorus sulfur chlorine solid electrolyte powder for use; 2. Set up 17 nozzles to prepare 4 layers of solid-state battery cells: Nozzle 1 uses selective laser sintering technology to print the bipolar current collector. After 1 to 2 minutes, nozzle 2 uses binder injection molding technology to print NCM811 powder on the current collector. After 1 to 2 minutes, nozzle 3 uses selective laser sintering technology to print solid electrolyte powder on the positive electrode layer. After 1 to 2 minutes, nozzle 4 uses binder injection molding technology to print lithium indium alloy powder on the solid electrolyte layer. Repeat the above preparation unit. A total of 17 layers are printed, from bottom to top, namely, bipolar current collector layer, positive electrode layer, solid electrolyte layer, negative electrode layer, bipolar current collector layer, positive electrode layer, solid electrolyte layer, negative electrode layer, bipolar current collector layer, positive electrode layer, solid electrolyte layer, negative electrode layer, bipolar current collector layer, positive electrode layer, solid electrolyte layer, negative electrode layer, bipolar current collector layer, positive electrode layer, solid electrolyte layer, negative electrode layer and bipolar current collector layer, and finally a solid-state battery cell block is obtained; when printing layer by layer, a roller is attached behind the printing nozzle of each layer, and roller pressing is performed immediately after printing, and the rolling pressure of a single layer is 10 MPa.
[0069] 3. The obtained solid-state battery cell block is subjected to isostatic pressing at a pressure of 500 MPa, a temperature of 25 degrees Celsius, and a time of 15 minutes; 4. Cut the block to obtain a solid-state battery cell with a size of 6 cm × 8 cm; 5. Weld the pole ears on both sides of the solid-state battery cell and encapsulate it with an aluminum-plastic film to obtain a finished battery cell.
[0070] Example 3
[0071] This embodiment provides a solid-state battery, the preparation of which includes: 1. Prepare stainless steel current collector powder, ternary positive electrode powder (including 80 parts of NCM811, 2 parts of super-p, 3 parts of polyvinylidene fluoride, 15 parts of lithium lanthanum zirconium oxide solid electrolyte), lithium / indium metal powder and lithium lanthanum zirconium oxide solid electrolyte powder for use; 2. Set up 17 nozzles to prepare 4 layers of solid-state battery cells: Nozzle 1 uses selective laser sintering technology to print the bipolar current collector. After 1 to 2 minutes, nozzle 2 uses binder injection molding technology to print NCM811 powder on the current collector. After 1 to 2 minutes, nozzle 3 uses selective laser sintering technology to print solid electrolyte powder on the positive electrode layer. After 1 to 2 minutes, nozzle 4 uses binder injection molding technology to print lithium indium alloy powder on the solid electrolyte layer. Repeat the above preparation unit. A total of 17 layers are printed, from bottom to top, namely, bipolar current collector layer, positive electrode layer, solid electrolyte layer, negative electrode layer, bipolar current collector layer, positive electrode layer, solid electrolyte layer, negative electrode layer, bipolar current collector layer, positive electrode layer, solid electrolyte layer, negative electrode layer, bipolar current collector layer, positive electrode layer, solid electrolyte layer, negative electrode layer, bipolar current collector layer, positive electrode layer, solid electrolyte layer, negative electrode layer and bipolar current collector layer, and finally a solid-state battery cell block is obtained; when printing layer by layer, a roller is attached behind the printing nozzle of each layer, and roller pressing is performed immediately after printing, and the rolling pressure of a single layer is 10 MPa.
[0072] 3. The obtained solid-state battery cell block is subjected to isostatic pressing at a pressure of 500 MPa, a temperature of 25 degrees Celsius, and a time of 15 minutes; 4. Cut the block to obtain a solid-state battery cell with a size of 6 cm × 8 cm; 5. Sinter the obtained solid-state battery cell at 1100 degrees Celsius for 6 hours. Weld the pole ears on both sides of the solid-state battery cell and package it with aluminum-plastic film to obtain a finished battery cell.
[0073] Figure 3 This is a process flow chart of 3D printing solid-state batteries provided in this embodiment.
[0074] Example 4
[0075] This embodiment provides a solid-state battery, the preparation of which is different from that of Embodiment 3 only in that no sintering step is included after cutting, and packaging is performed directly.
[0076] Example 5
[0077] This embodiment provides a solid-state battery, and the preparation method thereof is different from that of Embodiment 2 only in that sintering is performed after cutting, the sintering temperature is 200 degrees Celsius, the sintering time is 5 hours, and packaging is performed after sintering.
[0078] Example 6
[0079] This embodiment provides a solid-state battery, and the preparation method thereof is different from that of Embodiment 2 only in that the lamination pressure is 100 MPa.
[0080] Example 7
[0081] This embodiment provides a solid-state battery, and the preparation method thereof is different from that of Embodiment 2 only in that: during layer-by-layer printing, no single-layer rolling is performed.
[0082] Comparative Example 1 (Compared with Example 1)
[0083] This comparative example provides a solid-state battery, and its preparation method comprises the following steps: 1. Prepare stainless steel current collector powder, lithium iron phosphate positive electrode powder (including 70 parts of lithium iron phosphate powder, 2 parts of conductive carbon black, 2 parts of polytetrafluoroethylene, 26 parts of lithium titanium aluminum phosphate solid electrolyte), silicon carbon negative electrode powder (including 80 parts of silicon carbon powder, 1 part of conductive carbon black, 4 parts of polyvinyl pyrrolidone, 15 parts of lithium phosphorus sulfur chlorine solid electrolyte) and lithium phosphorus sulfur chlorine solid electrolyte powder for use; 2. Set up 1 nozzle to prepare 3 layers of solid-state battery cell blocks: first, use the selective laser sintering process to print the bipolar current collector. After the current collector is printed and completely solidified for 15 minutes, use the binder injection molding process to print the lithium iron phosphate positive electrode powder on the current collector. After the positive electrode is printed and completely solidified for 30 minutes, use the selective laser sintering process to print the solid electrolyte powder on the positive electrode layer. After the solid electrolyte is printed and completely solidified for 15 minutes, use the binder injection molding process to print the silicon-carbon negative electrode powder on the solid electrolyte layer. Repeat the above preparation unit to obtain a solid-state battery cell block; 3. The obtained solid-state battery cell block is subjected to isostatic pressing at a pressure of 500 MPa, a temperature of 25 degrees Celsius, and a time of 15 minutes; 4. Cut the block to obtain a solid-state battery cell with a size of 6 cm × 8 cm; 5. Weld the pole ears on both sides of the solid-state battery cell and encapsulate it with an aluminum-plastic film to obtain a finished battery cell.
[0084] Comparative Example 2
[0085] This comparative example provides a solid-state battery, and its preparation method is different from that of Example 1 only in that the bipolar current collector layer is not obtained by 3D printing, but is directly covered with a ready-made stainless steel foil.
[0086] Test Example 1
[0087] The present invention tests the performance and output voltage of the solid-state batteries prepared in the embodiments and comparative examples, and the results are shown in Table 1.
[0088] Detection methods include: Output voltage: Use a universal digital meter to measure the positive and negative voltages of the battery cell; Rate performance: The battery cell is charged and discharged to test the capacity retention rate at a 3 coulomb discharge rate; Production efficiency: the time taken to produce a single battery cell (unit: minutes).
[0089] Table 1
[0090] According to Table 1, by comparing Example 1 with Comparative Example 1, it can be seen that the 3D printing method described in this application can effectively ensure the battery performance while significantly improving the production efficiency by printing the entire battery cell block in an integrated manner; by comparing Example 1 with Comparative Example 2, it can be seen that, compared with directly performing 3D printing on the solid current collector plate of the finished product, the current collector is printed in an integrated manner, which can further increase the composite effect of the electrode material and the current collector, thereby enhancing the battery cell performance. By comparing Example 2 with Example 4, Example 5 and Example 7, it can be seen that when the preparation steps of the solid-state battery outside the scope of the present application are used, the performance of the battery cell will be affected.
[0091] It should be noted that, according to the 3D printing method of the present invention, the raw materials of the positive and negative electrodes and the solid electrolyte can be arbitrarily replaced with other raw materials specified in the present invention, which is equivalent to the effect of the embodiment.
[0092] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a solid-state battery, characterized in that: include: The entire solid-state battery cell is printed in an integrated manner using 3D printing to obtain a solid-state battery cell block; the solid-state battery cell block is then laminated; wherein the solid-state battery cell block includes a bipolar current collector layer, a positive electrode layer, a solid electrolyte layer, a negative electrode layer and a bipolar current collector layer from bottom to top.
2. The method for preparing a solid-state battery according to claim 1, characterized in that: When 3D printing solid-state batteries, each 3D printing nozzle corresponds to a raw material, and multiple layers are printed simultaneously; preferably, when 3D printing is performed, from bottom to top, the bipolar current collector layer is printed first, and the positive electrode layer is printed on the bipolar current collector layer 0.5 to 2 minutes later; then the solid electrolyte layer is printed on the positive electrode layer 0.5 to 2 minutes later, and then the negative electrode layer is printed on the solid electrolyte layer 0.5 to 2 minutes later, and then the bipolar current collector is printed on the negative electrode layer 0.5 to 2 minutes later, to achieve simultaneous printing of multiple layers, and after the printing is completed, it is a battery unit.
3. The method for preparing a solid-state battery according to claim 1, characterized in that: The lamination comprises a rolling or isostatic pressing process, and the lamination pressure is greater than 100 MPa.
4. The method for preparing a solid-state battery according to claim 3, characterized in that: During the 3D printing process, a single layer rolling is performed while printing each layer; preferably, the pressure of the single layer rolling is 5-15 MPa.
5. The method for preparing a solid-state battery according to any one of claims 1 to 3, characterized in that: The 3D printing process includes one or more of a binder jet printing process, a fused deposition printing process and a selective laser sintering printing process.
6. The method for preparing a solid-state battery according to claim 5, characterized in that: The positive electrode layer and the negative electrode layer are printed by the binder jetting process.
7. The method for preparing a solid-state battery according to claim 2, characterized in that: The raw material of the bipolar current collector layer includes stainless steel foil and / or aluminum-copper composite foil; And / or, the raw materials of the positive electrode layer include positive electrode active material, conductive agent, binder and solid electrolyte; preferably, the positive electrode active material includes lithium iron phosphate, lithium cobalt oxide, lithium nickel manganese oxide, ternary nickel cobalt manganese oxide or lithium-rich manganese base; the conductive agent includes one or more of super-p, conductive carbon black, acetylene black, graphene and carbon nanotubes; the binder includes polytetrafluoroethylene, polyvinyl pyrrolidone and / or polyvinylidene fluoride; And / or, the raw material of the solid electrolyte layer includes one or more of an oxide solid electrolyte, a sulfide solid electrolyte and a halide solid electrolyte; preferably, the oxide solid electrolyte includes one or more of lithium lanthanum zirconium oxide with a garnet structure, lithium lanthanum zirconium tantalum oxide with a garnet structure, lithium aluminum titanium phosphate with a NASICON structure and lithium aluminum germanium phosphate with a NASICON structure; the sulfide solid electrolyte includes one or more of lithium phosphorus sulfur chlorine, lithium germanium phosphorus sulfur, lithium tin phosphorus sulfur, lithium phosphorus sulfur and lithium tin sulfur; the halide solid electrolyte includes one or more of lithium indium chloride, lithium holmium chloride, lithium yttrium chloride, lithium scandium chloride and lithium erbium chloride; And / or, the raw material of the negative electrode includes one or more of graphite, silicon carbon, metallic lithium and lithium alloy.
8. The method for preparing a solid-state battery according to claim 7, characterized in that: When the raw material of the solid electrolyte layer is an oxide solid electrolyte, sintering is further performed after lamination, and the sintering temperature is 200-1100 degrees Celsius; and other solid electrolytes except the oxide solid electrolyte are not sintered after lamination.
9. The method for preparing a solid-state battery according to claim 8, characterized in that: include: S1: prepare bipolar current collector powder, positive electrode powder, negative electrode powder and solid electrolyte printing powder; S2: printing the entire solid-state battery cell in an integrated manner to obtain a solid-state battery cell block; during the 3D printing process, single-layer rolling is performed while printing each layer; S3: laminating the solid-state battery cell blocks; S4: Cut the laminated solid battery cell blocks according to the battery cell size requirements; S5: Encapsulating the cut battery cells to obtain solid-state battery cells connected in series; When the raw material of the solid electrolyte layer is an oxide solid electrolyte, the cutting further includes sintering, and the sintering temperature is 200-1100 degrees Celsius.
10. A solid-state battery, characterized in that: It is prepared by the preparation method of the solid-state battery according to any one of claims 1 to 9.
Citation Information
Cited By
Preparation method and application of lithium battery
CN119627244A
Composite positive plate as well as preparation method and application thereof
CN119695157A
Method for measuring relative density of solid-state battery, and solid-state battery and electric apparatus