Microwave-treated ultra-fast-cooled lithium-rich lithium manganese nickel oxide and method of making same
By sintering and quenching lithium-rich metal oxide materials, combined with microwave radiation thermal decomposition, cobalt-free lithium-ion battery cathode materials are prepared, which solves the problems of high cost and complicated supply chain of cobalt-containing materials in lithium-ion batteries, and achieves High specific capacity and robust battery electrochemical performance.
Patent Information
- Application Number
- CN202380019674.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-05
- Filing Date
- 2023-01-03
- Publication Date
- 2024-10-29
AI Technical Summary
The high cost and complex supply chain of cobalt-containing cathode materials in existing lithium-ion batteries has led to the need for a reliable cobalt-free cathode material for lithium-ion batteries.
By sintering and quenching the lithium-rich metal oxide material, Lix(MnyNi1-y)2-xO2 material with layered hexagonal phase and monoclinic phase is formed. Microwave radiation is used for thermal decomposition and rapid quenching to prepare a material with Cathode active materials with high specific capacity and robust performance.
It achieves high specific capacity and long-term stability, reduces the use of cobalt, avoids the complexity of the cobalt supply chain, and improves the electrochemical performance of the battery.
Smart Images

Figure CN118872084A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application is a continuation-in-part of U.S. patent application No. 17 / 810,722 filed on July 5, 2022, and claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 296,243 filed on January 4, 2022 and U.S. Provisional Patent Application No. 63 / 296,244 filed on January 4, 2022, the entire contents of which are incorporated herein by reference. Technical Field
[0003] Aspects of the present invention relate to cathode materials for lithium-ion batteries, and more particularly, to lithium-rich lithium nickel manganese oxide cathode active materials, and methods of making the same. Background Art
[0004] Cobalt-containing cathode materials in lithium-ion batteries account for a large portion of the cost of contemporary battery cells, and cobalt is a major contributor to the cost. The complexity of cobalt's supply chain makes it an unstable commodity. Therefore, reliable cobalt-free lithium-ion battery cathode materials are needed. Summary of the invention
[0005] According to various embodiments, a method includes sintering a lithium-rich metal oxide (LRMO) material at a sintering temperature to form a sintered LRMO material, and rapidly cooling the sintered LRMO material from the sintering temperature to room temperature in less than 500 milliseconds to form a lithium-rich metal oxide (LRMO) material having a chemical formula of Li x (Mn y Ni 1-y ) 2-x A quenched LRMO material represented by O2 (wherein x is greater than 1.05 and less than 1.25, and y is in the range of 0.95 to 0.1).
[0006] According to various embodiments, a method includes thermally decomposing a precursor material using microwave radiation to form a thermally decomposed lithium-rich metal oxide (LRMO) material, sintering the thermally decomposed LRMO material to form a sintered LRMO material, and quenching the sintered LRMO material to form a lithium-rich metal oxide having a chemical formula of Li x (Mn y Ni 1-y ) 2-x A quenched LRMO material represented by O2 (wherein x is greater than 1.05 and less than 1.25, and y is in the range of 0.95 to 0.1).
[0007] According to various embodiments, the cathode electrode active material is composed of the chemical formula Li x (Mn y Ni1-y ) 2-x O2 (wherein x is greater than 1.05 and less than 1.25, and y ranges from 0.95 to 0.1). The active material comprises a layered hexagonal phase and a monoclinic phase. The active material exhibits at least one of the following: (106) + (102): (101) x-ray diffraction peak intensity ratio greater than 0.32; when included in a lithium ion battery, provides a specific capacity of at least 165 mAh / g at a C / 20 rate during the first discharge; when included in a lithium ion battery, after 100 charge / discharge cycles, the average discharge voltage loss at a C / 20 rate is less than 10%; and / or when included in a lithium ion battery, 100 C / 5 charge / discharge cycles are performed with a capacity decay of less than 10%. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] The accompanying drawings, which are incorporated herein and constitute a part of this specification, illustrate example embodiments of the invention, and together with the general description given above and the detailed description given below, serve to explain the features of the invention.
[0009] Figure 1 are photographs of rapid quench systems according to various embodiments of the present disclosure.
[0010] Figure 2 Included are 4 consecutive video capture time-lapse images taken at 30 frames per second showing the rapid quenching process according to various embodiments of the present disclosure.
[0011] Figure 3 and Figure 4 To illustrate the Li according to various embodiments of the present disclosure x (Mn y Ni 1-y ) 2-x Figure 2. X-ray diffraction (XRD) patterns of O2 material (where x=1.2, and y=0.75) before and after rapid quenching, respectively.
[0012] Figure 5 To illustrate the Li of materials treated using only microwave heating of the sol-gel precursor material for 5 minutes according to various embodiments of the present disclosure. x (Mn y Ni 1-y ) 2-x Figure 2. X-ray diffraction pattern of an O2 material with x=1.16 and y=0.7.
[0013] Figure 6 To illustrate the Li treatment using microwave heating and ultra-rapid quenching according to various embodiments of the present disclosure x (Mn y Ni 1-y) 2-x Figure 2. X-ray diffraction pattern of an O2 material with x=1.16 and y=0.7.
[0014] 7A is a tunneling electron microscopy (TEM) atomic map micrograph of a prior art LRMO material that has not been subjected to rapid quenching prior to electrochemical cycling of the material.
[0015] Figure 7B TEM HAADF atomic map micrographs of LRMO materials subjected to rapid quenching prior to electrochemical cycling of the materials according to various embodiments of the present disclosure.
[0016] For Li that was neither microwaved nor rapidly quenched (in this case, relatively slowly cooled on a metal plate), x (Mn y Ni 1-y ) 2-x Comparative example of O2 material (where x=1.16, and y=0.7), Fig. 8A is a graph showing cell potential versus specific capacity, and Figure 8B is a plot of specific capacity versus cycling.
[0017] For an exemplary battery including a LRMO active material according to various embodiments of the present disclosure, Fig.9A To show a graph of cell potential versus specific capacity during break-in cycles, Fig. 9B To show a graph of cell potential versus specific capacity over time, Fig. 9C is a graph showing specific capacity versus cycle at C / 20 rate, and Fig.9D Graph showing the specific discharge capacity at C / 5 rate versus cycle number with a C / 20 reference cycle.
[0018] Fig. 10A To show that Li x (Mn y Ni 1-y ) 2-x Plot of cell potential versus specific capacity for a comparative cell of an O2 active material where x=1.16 and y=0.7, Fig. 10B To show Fig. 10A A graph of the specific capacity of a battery versus cycles.
[0019] Fig. 10C To show the Li x (Mn y Ni 1-y ) 2-xPlot of cell potential versus specific capacity for an exemplary cell with O2 active material where x=1.16 and y=0.7. Fig. 10D To show Fig. 10C A graph of the specific capacity of a battery versus cycles.
[0020] Fig.11A To illustrate the various embodiments of the present disclosure, Li x (Mn y Ni 1-y ) 2-x A graph of cell potential versus specific capacity for an exemplary cell with O2 active material where x=1.16 and y=0.7, and Fig. 11B To show Fig.11A Specific discharge capacity versus cycle for cells at C / 20 and C / 2 rates.
[0021] Fig. 12A To show that the formula Li[Ni x Li (1 / 3–2x / 3) Mn (2 / 3-x / 3) ]O2 (wherein the nickel content x = 0.25) lithium-rich nickel manganese oxide material sample during the cycle, and Figures 12B to 12D Shown are the full charge and discharge curves of coin cells containing 25 Hq, 25 Lq and 25 Mq samples respectively.
[0022] Fig.13A is a graph showing the specific discharge capacity of the x=0.17 sample during cycling, and Figures 13B to 13D Shown are the full charge and discharge curves of coin cells containing 17 Hq, 17 Lq and 17 Mq samples respectively.
[0023] Fig.14A is a graph showing the specific discharge capacity of the x=0.10 sample during cycling, and Figures 14B to 14D Shown are the full charge and discharge curves of coin cells containing 10 Hq, 10 Lq and 10 Mq samples respectively.
[0024] Figures 15A to 15I Graph showing normalized and shifted XRD patterns of LLRNMO powder before and after cycling for 25Hq, 25Lq, 25Mq, 17Hq, 17Lq, 17Mq, 10Hq, 10Lq and 10Mq samples, respectively.
[0025] Fig.16 Included are SEM micrographs at 50 k× of cathodes sprayed with 25Hq, 25Lq, and 25Mq samples before and after cycling.
[0026] Fig.17Included are SEM micrographs at 50 k× of cathodes sprayed with 17Hq, 17Lq, and 17Mq samples before and after cycling.
[0027] Fig.18 Included are SEM micrographs at 5k× of cathodes sprayed with 10Hq, 10Lq, and 10Mq samples before and after cycling.
[0028] Figures 19A to 19C Graph showing a smoothed spline fit of the dQ / dV vs. V data for the first charge cycle for the x=0.25, x=0.17, and x=0.10 samples.
[0029] Figures 20A to 20C Graph showing a smoothed spline fit of the dQ / dV vs. V data for the second charge cycle for the x=0.25, x=0.17, and x=0.10 samples.
[0030] Figures 21A to 21C is a graph showing the first C / 2 discharge and the last C / 2 discharge of the 25Hq, 25Lq and 25Mq samples, and Fig.21D Graph showing the average discharge voltage per cycle for the 25Hq, 25Lq and 25Mq samples during cycling.
[0031] Figures 22A to 22C is a graph showing the first C / 2 discharge and the last C / 2 discharge of the 17Hq, 17Lq and 17Mq samples, and Fig.22D Graph showing the average discharge voltage per cycle for the 17Hq, 17Lq and 17Mq samples during cycling.
[0032] Figures 23A to 23C is a graph showing the first C / 2 discharge and the last C / 2 discharge of the 10Hq, 10Lq and 10Mq samples, and Fig.23D Graph showing the average discharge voltage per cycle for the 10Hq, 10Lq and 10Mq samples during cycling.
[0033] Fig.24 Schematic diagram showing how phase impurity inclusions in a 25Mq sample with R-3m structure and lattice parameter a'>a give rise to secondary peaks as seen to the left of the 25Mq (104) peak.
[0034] Figures 25A to 25B is the SEM micrograph of the agglomerates, and Figures 25C to 25D is a higher magnification SEM micrograph of crystallites (eg, grains) in the agglomerates.
[0035] Fig.26AGraphs showing the intensity (in arbitrary units) versus the angle 2θ (in degrees) of the exponentially normalized and shifted XRD patterns of pristine layered lithium-rich nickel manganese oxide (LLRNMO) powder. Fig.26B Included are an upper graph showing the trend between the lattice parameter "a" and the nickel content of the sample obtained by single-phase Rietveld fitting, and a lower graph showing the trend between the lattice parameter "c" and the nickel content of the sample. DETAILED DESCRIPTION
[0036] As described herein, aspects of the present disclosure are described with reference to exemplary embodiments and / or drawings showing exemplary embodiments of the present invention. However, the present invention can be presented in many different forms and should not be construed as being limited to the exemplary embodiments shown in the drawings or described herein. It should be understood that a plurality of disclosed embodiments may include specific features, elements, or steps described in conjunction with the particular embodiment. It should also be understood that, although described with respect to a particular embodiment, specific features, elements, or steps may be interchanged or combined with alternative embodiments in a variety of combinations or arrangements not shown.
[0037] A number of embodiments will be described in detail with reference to the accompanying drawings. Wherever possible, the same reference numerals will be used throughout the drawings to refer to the same or similar parts. Reference to specific examples and implementations is for illustrative purposes and is not intended to limit the scope of the invention or claims.
[0038] Ranges may be expressed herein as from "about" one particular value and / or to "about" another particular value. When such ranges are expressed, examples include from a particular value and / or to another particular value. Similarly, when a value is expressed as an approximation by using the antecedent "about" or "substantially," it is understood that the particular value constitutes another aspect. In some embodiments, a value of "about X" may include a value of + / -1% X. It is also understood that the endpoints of each range are important relative to and independent of the other endpoint.
[0039] According to various embodiments, methods are provided for rapidly and inexpensively forming crystallographically stable, highly durable, cobalt-free, lithium-rich metal oxide (LRMO) materials. In some embodiments, the LRMO material may be a lithium-rich lithium manganese nickel oxide material represented by the following general formula 1:
[0040] Li x (Mn y Ni 1-y ) 2-x O2 (Formula 1),
[0041] Wherein x is greater than 1.0 and less than 1.25, and y ranges from 0.95 to 0.1, such as about 0.8 to 0.5.
[0042] In some embodiments, the LRMO material may be a lithium-rich lithium manganese nickel oxide material represented by Formula 2 below:
[0043] Li[Li (1 / 3-2x / 3) Mn (2 / 3-x / 3) Ni x ]O2 (Formula 2)
[0044] where x ranges from 0.1 to 0.4.
[0045] The LRMO material in its original state (e.g., before the first charge) can have different hexagonal (e.g., rhombohedral) and monoclinic phases. Therefore, the LRMO material can be represented by the expression (1-x)[Li2MnO3]*x[LiMn a Ni (1-a) O2], wherein the first part of the expression represents the relative molar amount of the monoclinic phase (1-x), and the second part of the expression represents the relative molar amount of the rhombohedral phase (x). The mole fraction "x" of the rhombohedral phase generally ranges from 0.8 to 0.95, while "a" ranges from 0.6 to 0.9. In some embodiments, the two phases may be arranged in a layered structure.
[0046] Various embodiments provide LRMO materials that exhibit high (eg, >240 mAh / g) specific capacity and high functional voltage window (eg, 2.0 V to 4.8 V) when used as active materials for cobalt-free cathodes.
[0047] According to various embodiments, the method of forming the LRMO material includes rapid thermal processing and rapid (e.g., less than 10 seconds) or ultra-rapid (e.g., less than 500 milliseconds) quenching, which produces an LRMO material having an excellent crystal structure with desired atomic order / disorder. These features can provide unexpectedly robust long-term stability and performance when used as a cathode active material.
[0048] Conventional LRMO materials are generally unsuitable for use as cathode active materials due to their low rate capabilities and poor capacity retention, which are believed to be caused by structural instability due to oxygen loss, transition metal ion migration during use, and possible manganese dissolution. The two most common aging mechanisms are manifested by average discharge voltage decay as the material slowly reorganizes into a dominant spinel structure, and capacity loss after cycling due to mechanical and / or chemical degradation of the material.
[0049] Thermal decomposition and treatment
[0050] LRMO materials can be synthesized from precursor materials by a variety of methods. Table 1 below includes specific methods that can be used to synthesize LRMO materials, including precursor synthesis, precursor materials, quenching methods, performance indicators and discharge capacity (DC) of LRMO material cathodes.
[0051] Table 1
[0052]
[0053] As shown in Table 1, the three main synthetic routes of LRMO materials include precipitation followed by combustion, hydrothermal synthesis, and sol-gel solution production followed by moderate-temperature decomposition and high-temperature heat treatment (e.g., calcination, annealing, sintering).
[0054] As can be seen in Table 1, the number of studies exploring the effect of nickel composition on the performance of LRMO cathodes has decreased over time; few studies have explored the effects of nickel composition on the performance of LRMO cathodes with the formula Li[Ni x Li (1 / 3–2x / 3) Mn (2 / 3-x / 3) ]O2 cathodes or nickel compositions below x = 0.2. Table 1 also shows that there are significant inconsistencies in the synthesis routes used between studies. In addition, there are few studies that conduct detailed comparative assessments of the effects of synthesis methods on LRMO cathode performance. In LRMO materials, transition metal order and disorder may be important, and both composition and synthesis techniques may provide mechanisms that affect the degree of structural order and disorder. The electrochemical behavior that these compositional and synthetic variations may cause (e.g., different defect concentrations), for example, may have a significant impact on the properties of LRMO cathodes.
[0055] Without wishing to be bound by a particular theory, it is believed that when the sample is quenched in liquid nitrogen, the particles are immediately shielded by an insulating blanket of nitrogen, similar to the Leidenfrost effect, which significantly reduces the heat transfer rate. It is believed that in the prior art, lithium-containing cathode materials for lithium-ion batteries are not allowed to come into contact with moisture because water causes lithium to seep out of such cathode materials and form a lithium hydroxide coating on the material. Furthermore, water is known to cause failure of lithium-ion batteries, such as lithium-ion batteries containing lithium iron phosphate cathode materials.
[0056] While not wishing to be bound by a particular theory, the inventors believe that the relatively slow conventional quenching and cooling processes result in agglomeration of the metal oxides, thereby forming separate nickel oxide and lithium manganese oxide phases. In particular, the nickel oxide phases may be concentrated on the surface of the LRMO material particles (e.g., crystallites). This surface nickel oxide agglomeration is believed to be at least partially responsible for the chemical instability of conventional LRMO active materials.
[0057] In contrast, the present inventors unexpectedly determined that water quenching does not negatively affect LRMO cathodes and does not cause lithium to seep out of such LRMO cathodes. It is believed that water quenching causes evaporation in the form of bubble nucleation and dissipation, which actually increases the heat transfer rate. Therefore, it is believed that water quenching should have a heat transfer rate that can be approximated to be two orders of magnitude greater than liquid nitrogen quenching. In addition, both water and additives solvated therein (i.e., other materials that can be dissolved in water) can react with the high temperature LRMO upon high temperature LRMO quenching to produce favorable surface terminations and / or coatings, which enhance electrochemical stability and durability when used in lithium ion batteries.
[0058] In addition, in many prior art quenching routes mentioned above, quenching is carried out on the pressed sintering or partially sintered pellets of the complete material as a larger object (e.g., with a width of the order of centimeters). In contrast, in the embodiments of the present disclosure, loose and / or ground powders are quenched, and the powders have particles in shape that are agglomerates with an average diameter of 20 microns or less (e.g., an average diameter of 0.1 micron to 20 microns, such as 0.1 micron to 1 micron or 1 micron to 20 microns), so that when the particles contact the quenching liquid (e.g., water), all materials are rapidly cooled at approximately the same rate. Each agglomerate is composed of crystallites with an average size range of about 25nm to about 500nm, such as 50nm to 200nm. Each crystallite can include a single crystal of LRMO material. Crystallites can be partially fused together in agglomerates or completely fused together in agglomerates. If the crystallites are completely fused in the agglomerate (i.e. in the powder particles), each crystallites comprises a single grain of the powder particles, which is separated from other single grains in the same powder particles by grain boundaries. The average grain size of the powder particles may range from about 25 nm to about 500 nm, for example 50 nm to 200 nm. Agglomerates may be relatively porous, which allows water to reach the crystallites inside the agglomerates.
[0059] Fast and ultra-fast cooling
[0060] According to various embodiments, the LRMO cathode active material can be formed by heat treating (e.g., sintering, calcining and / or annealing) and quenching the LRMO material powder. In particular, the heat treatment may include a high temperature process in which the LRMO material may be heated to a process temperature in the range of about 800°C to about 1000°C, for example, about 850°C to about 950°C, or about 900°C. The heat treatment may be performed in any suitable heat treatment equipment, such as a furnace, such as a tube furnace, a muffle box furnace, and the like. In some embodiments, the heat treatment may optionally include one or more low temperature precursor decomposition (e.g., firing) processes in which the LRMO material is heated to a temperature above room temperature and below 800°C. For example, firing may include heating the LRMO material to a temperature in the range of about 450°C to about 550°C, for example, about 500°C, prior to the high temperature process.
[0061] According to various embodiments, the quenching process may include transferring the heated LRMO material to a quenching bath. For example, the LRMO material may be placed directly into a quenching bath from a thermal treatment apparatus.
[0062] In prior art methods, the LRMO material may be slowly cooled during transfer from the furnace. For example, the transfer process may take about 10 seconds, during which the temperature of the LRMO material may slowly decrease. The inventors have determined that slow cooling prior to entering the quench bath may result in undesirable changes in the crystal structure of the sintered LRMO material. In other words, the temperature of the sintered LRMO material entering the quench bath may be important in providing a desired crystal structure. For example, slow cooling may result in a less desirable crystal structure.
[0063] According to various embodiments, the transfer process can be configured such that the sintered LRMO material enters a quench bath at a temperature of at least 800°C, such as a temperature in the range of 800°C to 950°C, or about 850°C to about 925°C, or about 900°C after the sintering process. For example, the transfer time from the heat treatment device to the quench bath can be limited to 10 seconds or less, such as 1 second or less, such as less than 0.5 seconds, or 0.2 seconds or less. Thus, the sintered LRMO material is cooled from the heat treatment temperature (e.g., from a sintering temperature of at least 800°C, such as a temperature in the range of 800°C to 950°C, or about 850°C to about 925°C, or about 900°C) to room temperature (e.g., 25°C) in 10 seconds or less, such as less than 0.5 seconds, including 0.2 seconds or less. Herein, an "ultra-fast quenching process" may have a cooling time of less than 0.5 seconds, such as 0.2 seconds or less, such as 0.1 seconds to 0.2 seconds, and a "fast quenching process" may have a cooling time of 10 seconds or less, such as 0.5 seconds to 10 seconds.
[0064] The sintered LRMO powder particles can be quenched in a quench bath at an average rate of at least 50°C / sec, such as 50°C / sec to 10,000°C / sec. For example, the sintered LRMO powder particles can be quenched at a rate of 87.5°C / sec to 8750°C / sec, such as at least 1750°C / sec, such as 1750°C / sec to 8750°C / sec, including 4375°C / sec to 8750°C / sec. Thus, the sintered LRMO material can be quenched from a temperature between a heat treatment temperature of at least 800°C (e.g., a sintering temperature) to a temperature of a quench bath (e.g., a room temperature water bath at 25°C) in 10 seconds or less, such as in less than 500 milliseconds, including 400 milliseconds or less, 300 milliseconds or less, or 200 milliseconds or less. For example, quenching can occur in 100 milliseconds to 400 milliseconds or 100 milliseconds to 200 milliseconds.
[0065] The quench bath may contain a high heat capacity liquid solvent having an evaporation temperature of less than about 200° C. For example, the quench bath may contain a solvent such as water, oil, and / or alcohol. In some embodiments, the quench bath may contain an additive configured to modify the surface of the LRMO material during quenching to improve the long-term chemical stability of the material. The additive may include an acid, an alcohol, and / or a dissolved carbon material, such as an acid, an alcohol, or a carbon material dissolved in water.
[0066] For example, the quench bath can be an aqueous quench solution comprising about 0.01 mol / L to about 1.0 mol / L, such as about 0.1 mol / L to 1.0 mol / L, or about 0.5 mol / L to 1.0 mol / L of an acid additive, such as sulfuric acid, hydrochloric acid, nitric acid, oxalic acid, citric acid, acetic acid, phosphoric acid, orthophosphoric acid, combinations thereof, etc. The acid can be configured to stabilize the surface of the LRMO particles by reacting with and / or passivating dangling bonds and / or OH end groups of the LRMO powder particles quenched in water comprising the acid additive.
[0067] In some embodiments, acid quenching can cause a spinel structure (e.g., a surface layer) to form on the surface of the quenched LRMO powder particles. The spinel structure can form a framework that stabilizes the particles and provides a three-dimensional path for lithium diffusion. In particular, it is believed that the acid can cause the Li ions of the particles to exchange with the H ions of the acid, and subsequent structural transformation of the particle surface, thereby forming a spinel surface layer.
[0068] In another embodiment, in addition to or in place of the acid additive, the quenching solution may include an alcohol and / or a carbohydrate additive. For example, the alcohol may include isopropanol or another alcohol, and the carbohydrate may include a sugar, such as fructose, galactose glucose, lactose, maltose, sucrose, a combination thereof, and the like. In some embodiments, the quenching solution may include about 0.01 mol / L to about 1.0 mol / L, such as about 0.1 mol / L to 1.0 mol / L, or about 0.5 mol / L to 1.0 mol / L of a carbohydrate additive. During the quenching process in water containing carbohydrate particles, the carbohydrate may form a tight amorphous carbon coating on the surface of the LRMO powder particles. The carbon coating may be permeable to Li ions, but may be impermeable to the electrolyte of the Li ion battery. The carbon coating may also allow volume changes of the LRMO crystallites to occur during charging and discharging of the battery.
[0069] A rapid or ultra-rapid quenching process can produce a quenched LRMO material having a crystal structure that provides unexpected robustness and electrical properties. Specifically, the degree of crystalline order in a quenched LRMO material (e.g., lithium-rich lithium manganese nickel oxide) produced by a quenching process can provide performance characteristics suitable for use as a cathode active material for a lithium-ion battery, the cathode active material providing energy density and charge storage stability characteristics similar to cathodes comprising cobalt-containing, high nickel content active materials.
[0070] The quenching process can produce a quenched LRMO material powder having a desired crystal structure and particle size. For example, the quenched sintered LRMO material can be a loose powder with an average particle size of about 1 μm or less, such as an average particle size range of about 0.02 μm to about 1 μm, or about 0.05 μm to about 0.5 μm. In some embodiments, the quenched LRMO material may include a crystalline phase and / or crystallites with an average crystal size range of about 25 nm to about 500 nm, such as about 50 nm to about 300 nm. Each powder particle may include one crystallite or more than one crystallite. Loose sintered and quenched powder particles can be incorporated into a binder (e.g., a carbon binder) to form a cathode electrode for a Li-ion battery.
[0071] The quenched LRMO material is dried to form an LRMO active material (e.g., heat treated and quenched loose powder particles), which may have a hexagonal primary phase and a monoclinic secondary phase. Thus, the ratio of the hexagonal phase content to the monoclinic phase content is greater than 1, such as at least 2, such as 2 to 20. For example, the sintered and quenched LRMO material (e.g., dried active material) may have a superlattice structure comprising hexagonal primary phase layers separated by interlayers of the monoclinic secondary phase. Alternatively, the sintered and quenched LRMO material may include a hexagonal phase matrix comprising monoclinic phase nanodomains (i.e., regions having a width of less than one micron). Mn and Ni may be uniformly distributed in the crystal structure of the LRMO material (e.g., excess Mn, Ni, and Li are uniformly and consistently distributed on transition metal lattice sites). For example, a sintered and quenched crystalline grain of LRMO material exhibits a uniform distribution of Mn and Ni atoms throughout the crystalline grain, such that when imaged by high angle annular dark field (HAADF) energy dispersive X-ray spectroscopy (EDS) (i.e., in an EDS elemental map of a HAADF tunneling electron microscopy image), there are no Ni-rich or Mn-rich regions. In one embodiment, the term "no Ni-rich or Mn-rich regions" in a crystalline grain means that there is no crystal volume greater than 3×3×3 nm in the crystalline grain in which the ratio of Ni and Mn atoms differs by more than 3% from the average ratio of Ni and Mn atoms in the entire crystalline grain.
[0072] The crystal structure of the active LRMO material thus formed may change due to electrochemical cycling. For example, when the active LRMO material is included as an active material in an electrochemical cell, the monoclinic phase may no longer be present at a detectable level after the first charge / discharge cycle. It is believed that the monoclinic phase may be consumed during Li ion insertion and / or deinsertion.
[0073] Rapid precursor decomposition
[0074] LRMO materials can be formed from various precursor materials. For example, the precursor material can be a metal organic compound containing a metal (e.g., Li, Mn, and / or Ni) and a solubilizing agent (e.g., an organic ligand). For example, the precursor material can include a metal acetate, a metal carbonate, a metal nitrate, a metal sulfate, and / or a metal hydroxide.
[0075] In various embodiments, the LRMO material can be formed by thermally decomposing a precursor material and then sintering and quenching the resulting thermally decomposed LRMO material. The precursor material may include a gel formed via a sol-gel process. The inventors have determined that rapidly decomposing the precursor material gel can improve the uniformity of the LRMO material. For example, in the sol portion of the sol-gel process, stoichiometric amounts of precursors containing Li, Mn, and Ni can be mixed with water to form an aqueous mixture. For example, stoichiometric amounts of Li(CH3COO)*2H2O, Mn(CH3COO)2*4H2O, and Ni(NO3)2*6H2O can be mixed to form an aqueous mixture. However, the present disclosure is not limited to any particular precursor material. For example, in some embodiments, all acetate precursors or all nitrate precursors (i.e., lithium nitrate, manganese nitrate, and nickel nitrate) can be used. In some embodiments, the mixture may contain an excess of 0.01 to 0.20 mole fraction of lithium acetate precursor to compensate for lithium loss during processing.
[0076] The mixture may then be heated to form a precursor gel.For example, the mixture may be heated at a temperature in the range of about 90°C to about 150°C, such as about 100°C, for a period of time sufficient for gelation to occur.
[0077] The gel can then be thermally decomposed. For example, the gel can be heated at a temperature and for a period of time sufficient to remove (e.g., volatilize and / or decompose) the solubilizing agent (e.g., organic ligand) and / or solvent of the gel and form a thermally decomposed LRMO material.
[0078] Thermal decomposition can be performed using conventional furnaces such as muffle box furnaces and / or tube furnaces. However, such devices typically have slow heating and cooling rates of about 1°C to 10°C per minute and do not employ any type of direct radiant heat energy input. Therefore, conventional furnaces may require at least 8 hours of processing time and a large amount of energy to form a thermally decomposed LRMO material.
[0079] According to various embodiments, a rapid (e.g., high rate) heating method is used to form a thermally decomposed LRMO material. For example, one embodiment may utilize microwave radiation to thermally treat the LRMO precursor material (i.e., rapidly decompose the LRMO precursor, such as a gel precursor formed via a sol-gel process).
[0080] Microwaves are defined as electromagnetic radiation with a wavelength of 1 mm to 1 m. Widely used household microwave ovens use microwave radiation with a frequency of about 2.45 GHz. Regulations have limited the microwave frequencies that can be used for domestic and industrial applications. The mechanism of microwave heating is attributed to two categories: 1) the flow of electric current under the external electric field generated by microwave radiation generates heat due to the Ohmic effect; and 2) dipoles present in the ceramic reorient themselves under the changing electric field, generating heat due to friction.
[0081] Microwave heating can allow lower thermal processing (e.g., precursor thermal decomposition) temperatures. Microwave heating can also allow shorter heating times compared to conventional furnace heating processes due to very rapid local heating. Intimate mixing of precursor materials can also allow more efficient volumetric heating than conventional furnace heating processes.
[0082] In some embodiments, microwave heating is used to heat and decompose the precursor material and form a thermally decomposed LRMO material. For example, the precursor material may contain ligands and / or metals that are highly sensitive to microwave radiation. Therefore, various embodiments utilize microwave radiation to heat the precursor and / or precursor gel to a very high temperature in a very short period of time. It has also been found that microwave heating also provides highly uniform heat distribution. Therefore, the use of microwave radiation can significantly change the heating rate and the resulting thermally decomposed LRMO material organization and / or structure. For example, microwave heating of the precursor gel can produce a highly uniform thermally decomposed LRMO material. The thermally decomposed LRMO material can be in the form of an inorganic ash that does not contain organic components (e.g., does not contain carbon or contains an unavoidable amount of carbon). Therefore, microwave heating can allow the formation of a thermally decomposed LRMO material without the need for a separate furnace firing (which can be omitted).
[0083] For example, the precursor gel can be provided to a microwave oven, where microwave radiation is used to decompose the gel and form a thermally decomposed LRMO material. For example, microwave radiation can be used to heat the gel to a temperature of at least 350°C, such as a temperature ranging from about 350°C to about 500°C for a period of time sufficient to volatilize the ligands and / or solvents of the gel and form a thermally decomposed LRMO material (e.g., LRMO inorganic ash). In various embodiments, continuous microwaves or pulsed microwaves with a power level of 20,000 W / kg of microwave material or less can be used to form a thermally decomposed LRMO material in about 30 minutes or less, such as in about 15 minutes to 30 minutes. Therefore, in order to form a thermally decomposed LRMO material with improved structural properties such as a uniform distribution of cations and / or metal oxides, the microwave-based heating process can be configured to quickly remove (e.g., evaporate and / or burn) organic components from the precursor material.
[0084] Although the microwave thermal decomposition of the precursor gel formed by the sol-gel process is described above, in other embodiments, the precursor by microwave thermal decomposition can also be formed by other methods. For example, alternative precursor preparation methods can include mechanical grinding / mixing methods, freeze-drying rotary evaporation or coprecipitation methods. In one embodiment of the coprecipitation method, a precursor comprising a hydroxide of Mn and Ni can be mixed with lithium carbonate and coprecipitated. For example, a solid precursor material comprising Li2CO3 or LiOH, nickel oxide and manganese oxide can also be used. Such a solid precursor can also have an excess of excess Li-containing precursor (e.g., lithium carbonate or lithium hydroxide) in an excess of 0.01 to 0.20 mole fraction to overcome the loss of lithium content during treatment. The precursor prepared by any of these methods can also be subjected to microwave thermal decomposition to form a thermally decomposed LRMO material (i.e., LRMO inorganic ash).
[0085] The thermally decomposed LRMO material (i.e., LRMO inorganic ash) can then be mixed and ground (e.g., milled) to form a precursor LRMO powder. The precursor LRMO powder is then heat treated (e.g., sintered) in any suitable heat treatment equipment (e.g., in a furnace, such as a tube furnace, a muffle box, etc.) to form a sintered LRMO material. For example, the precursor LRMO powder material can be heated (e.g., sintered) at a heat treatment temperature (e.g., a temperature of at least 800° C., such as about 900° C.) for a period of time ranging from about 12 hours to about 24 hours, and the sintered LRMO material can then be rapidly or ultra-rapidly quenched as described above to form a quenched LRMO material. The quenched LRMO material can then be dried and optionally re-ground (e.g., milled) into a LRMO active material (e.g., an active cathode material powder). The LRMO active cathode material powder can then be mixed with a binder or other inactive cathode material to form a cathode of a Li-ion battery.
[0086] According to various embodiments, methods of forming LRMO materials may include a combination of rapid heating (e.g., microwave heating) for at least a portion of the thermal treatment together with rapid or ultra-rapid quenching to produce LRMO materials with unexpectedly high performance. Specifically, the process can produce LRMO materials with a high degree of atomic / cation disorder / uniformity (which can be quantified using X-ray diffraction) while having no or substantially no surface segregation of nickel or nickel oxide in the particles (e.g., crystallites) (which can be observed using transmission electron microscopy). The combination of these material attributes produces a cathode active material that exhibits little to no capacity fade over 100 to 1000 charge / discharge cycles, significantly reduces or eliminates the loss in average discharge voltage during cycling, and exhibits rate performance suitable for commercial use.
[0087] According to various embodiments, embodiment methods including microwave heating and / or rapid / ultra-rapid quenching steps can be used to form LRMO active materials that do not suffer from the chemical instability of prior art LRMO materials. In particular, a rapid or ultra-rapid quenching step can be used to form a LRMO active material with reduced Ni surface segregation and increased structural uniformity compared to conventional LRMO materials that are slowly cooled after sintering. In various embodiments, the above microwave heating process can be used in combination with rapid or ultra-rapid quenching to form the LRMO active material. For example, a thermally decomposed LRMO material formed using microwave decomposition can be sintered and then subjected to a rapid or ultra-rapid quenching process.
[0088] In one embodiment, the cathode electrode (i.e., the positive electrode) comprises a LRMO active material comprising a powder embedded in a binder. The powder may have an average particle / agglomerate size ranging from about 0.1 μm to about 10 μm and an average crystal (i.e., crystallite) size ranging from about 25 nm to about 500 nm. In one embodiment, the particles of the LRMO active material powder may have at least one of a spinel surface layer, a carbon coating (e.g., produced by a carbohydrate additive in a quench bath), and / or a passivated oxygen bond (e.g., produced by an acid additive in a quench bath) on the surface. The cathode electrode may be included in a battery, such as a lithium ion battery, which also includes an anode electrode (i.e., a negative electrode), an electrolyte, and a separator.
[0089] In one embodiment, the cathode electrode active material may be composed of the chemical formula Li x (Mn y Ni 1-y ) 2-xO2 (wherein x is greater than 1.05 and less than 1.25, and y is in the range of 0.95 to 0.1). At least before subjecting a battery comprising the cathode electrode to a first electrochemical cycle, the active material may comprise a layered hexagonal (e.g., rhombohedral) phase and a monoclinic phase. The active material may exhibit at least one of the following: (i) (106) + (102): (101) x-ray diffraction peak intensity ratio greater than 0.32, for example, 0.33 to 0.346; and / or (ii) (003) to (104) x-ray diffraction peak ratio greater than 2, for example, 2.01 to 2.575; and / or (iii) when the cathode electrode is included in a lithium ion battery, at first discharge (e.g., at a C / 2 rate), provides at least 200 mAh / g, for example, 200 mAh / g to 230 mAh / g specific capacity; and / or (iv) when the cathode electrode is included in a lithium ion battery, the lithium ion battery exhibits an average discharge voltage loss of less than 10% at a C / 20 rate after 100 charge / discharge cycles; and / or (v) when included in the positive electrode of a lithium ion battery, at least 100 charge / discharge cycles, such as 200 C / 5 charge / discharge cycles, have a capacity fade of less than 10%, such as less than 5% (e.g., 0% to 4% capacity fade or capacity increase). In one embodiment, the lithium ion battery may include lithium or graphite as the anode electrode.
[0090] In one embodiment, the average discharge voltage of a battery (e.g., a lithium-ion battery) decreases by no more than 5% (e.g., 0% to 4%) after 50 C / 20 (charge)-C / 2 (discharge) charge / discharge cycles; and / or the discharge capacity of the battery is greater than 80% of its original capacity after 800 C / 20-C / 2 charge / discharge cycles.
[0091] Experimental example
[0092] The following method was used to produce Li x (Mn y Ni 1-y ) 2-xO2 (where x = 1.16 and y = 0.7). In particular, the precursor material gel is produced using a sol-gel solid-state synthesis method. The synthesis of the sol includes forming an aqueous mixture containing stoichiometric amounts of Li(CH3COO)*2H2O, Mn(CH3COO)2*4H2O and Ni(NO3)2*6H2O. The mixture is heated at 100°C until a gel is formed. The gel is poured into an alumina crucible and then fired at 400°C for 90 minutes to obtain an ash free of organic matter. The resulting ash is ground and fired again in a crucible at 500°C for 3 hours, then allowed to cool naturally before re-grinding, after which the powder is sintered at 900°C for 24 hours before quenching. All sintering is carried out in a box furnace under ambient fume hood conditions. All quenching is carried out after heating at 900°C for 12 to 24 hours.
[0093] Figure 1 is a photograph of a rapid quenching system 100 according to various embodiments of the present disclosure. Figure 2 Included are 4 consecutive video capture time-lapse images taken at 30 frames per second showing the rapid quenching process according to various embodiments of the present disclosure.
[0094] Reference Figure 1 and Figure 2 , the LRMO material is provided to a tube furnace 110, where the material is heated to 900°C. The heated LRMO material is output from the tube furnace 110 and quenched to room temperature in a quench bath 120. The tube furnace 110 rotates while in operation so that its contents are immediately dumped into the quench bath 110. The time period between the time the LRMO material leaves the furnace 110 at 900°C and the time it is quenched to room temperature takes less than 500 milliseconds, for example less than 200 milliseconds, to form the LRMO active material. After quenching, the LRMO material is filtered out of the water in the quench bath 120 and dried in a vacuum furnace.
[0095] In the first comparative example, the LRMO material was slowly cooled in the furnace 110 after being sintered at 900° C. In the second comparative example, the LRMO material was cooled by pouring onto a metal plate after sintering. In the third comparative example, the LRMO material was first slowly cooled to room temperature and then inserted into the tube furnace 110 for an ultra-rapid quenching step, and the LRMO material was kept at 900° C. for 30 to 120 minutes before the ultra-rapid quenching step.
[0096] In an alternative example, a rapid precursor decomposition process is used to form the LRMO powder. In particular, the above-described sol-gel precursor material is decomposed using microwave radiation to form a LRMO powder having an improved component distribution. In particular, the application of microwave radiation causes rapid volatilization of the organic components of the precursor material due to absorption of microwave energy by the organic components. Thus, due to the thermal energy generated by the microwave radiation, the LRMO components are uniformly mixed at the molecular level. The resulting LRMO powder is then sintered at 900° C. for 12 to 24 hours, followed by ultra-rapid quenching as described above.
[0097] Multiple larger batches (up to 1 kg) of cathode material were produced both with and without microwave decomposition and ultra-rapid quenching.
[0098] Material characterization
[0099] Figure 3 and Figure 4 is Li according to various embodiments of the present disclosure x (Mn y Ni 1-y ) 2-x Figure 2. X-ray diffraction (XRD) pattern of an O2 material with x=1.2 and y=0.75. Figure 3 The XRD patterns in the figure are produced by layered LRMO active materials that have not been rapidly quenched by immersion in water. Figure 4 The XRD patterns in FIG. 5 are produced by a layered LRMO active material that was rapidly quenched by immersion in water.
[0100] Evaluation of the XRD patterns revealed that the LRMO materials possess the expected hexagonal (e.g., rhombohedral) phase with a LiNiO2-related space group (R-3m) and a monoclinic phase with a Li2NiO3-related space group (C2 / c).
[0101] Figure 5 To illustrate the Li ions treated using microwave heating of the sol-gel precursor material for 5 minutes prior to the high temperature firing step according to various embodiments of the present disclosure. x (Mn y Ni 1-y ) 2-x Figure 1 shows the X-ray diffraction results of O2 material (where x=1.16 and y=0.7). Figure 5 Of greatest interest is the fact that this microwave decomposed material has a resulting x-ray diffraction pattern consistent with a highly crystalline and optimized material, including a rhombohedral LiNiO2-related space group (R-3m) and a monoclinic Li2NiO3-related space group (C2 / c). Thus, this material is suitable for forming LRMO using a 900°C anneal and rapid and / or ultra-rapid quench, as described above.
[0102] Figure 6 To illustrate the Li treatment using microwave heating and ultra-rapid quenching according to various embodiments of the present disclosure x (Mn y Ni 1-y ) 2-x Figure 1 shows the X-ray diffraction results of O2 material (where x=1.16 and y=0.7). Figure 6 , all expected peaks are present and well defined.
[0103] Fig. 7A is a prior art example from the literature (H. Zheng et al., "Recent developments and challenges of Li-rich Mn-based cathode materials for high-energy lithium-ion batteries", Materials Energy Today, Vol. 18, December 2020, p. 100518) of a tunneling electron microscopy (TEM) high-angle annular dark field imaging (HAADF) atomic map micrograph of the material before electrochemical cycling of a typical LRMO material that has not been subjected to rapid quenching. As can be seen from these micrographs, the initial LRMO material has significant nickel and manganese segregation inside the particles.
[0104] Figure 7B TEM HAADF atomic map micrographs of the produced LRMO material subjected to rapid quenching before electrochemical cycling according to various embodiments of the present disclosure. As can be seen from these micrographs, the LRMO material has no significant nickel / manganese segregation in the particles. Thus, rapid or ultra-rapid quenching reduces or eliminates nickel segregation on the particle surface, and nickel and manganese are uniformly mixed in the bulk of the LRMO material.
[0105] Crystalline homogeneity, cation disorder, and surface passivation
[0106] One method of assessing the degree of disorder of metal cations in a material is to use the ratio of peak intensities in an x-ray diffraction pattern. Specifically, the ratio of the intensity of the (003) peak to the (104) peak is generally considered to be a rough measure of electrochemical activity in mixed cation materials having such a predominantly layered crystal structure, while the ratio of the sum of the intensities of the (006) and (102) peaks to the intensity of the (101) peak is an indicator of cation disorder. Based on this, materials that are both microwave treated during the decomposition phase and then ultrafast quenched provide significantly higher electrochemical activity indicators and lower cation order (and therefore higher cation disorder) than slowly cooled materials.
[0107] Table 2 XRD peak ratio
[0108]
[0109] Table 2 shows the XRD peak intensity ratios of the comparative LRMO material (row 1) subjected to slow quenching after sintering and the exemplary LRMO material (row 2) subjected to ultra-rapid quenching after sintering. Both materials have the formula Lix(MnyNi1-y)2-xO2, where x=1.2, and y=0.75. Importantly, the exemplary ultra-rapid quenched material exhibits XRD features showing an increase in atomic disorder in the material, which has significantly higher electrochemical activity and greater cation disorder / metal oxide uniformity than the comparative material. Specifically, the exemplary material shows an increase in the ratio of the sum of the intensities of the (006) and (102) peaks to the intensity of the (101) peak, in this case about 9%. This significant increase in cation disorder represents a situation where the Ni and Mn atoms are more completely mixed (and therefore not aggregated) in the material. For this reason, such exemplary materials may be referred to as "cationically disordered lithium-rich lithium manganese nickel oxides," and these data demonstrate that different states of matter may be produced based on the processing conditions used, particularly the cooling rate used.
[0110] Electrochemical testing
[0111] The synthesized cathode material was mixed with Super-P carbon black and polyvinylidene fluoride (PVDF) in a ratio of 8:1.2:0.8, making the active material 80% of the total mass. The resulting blend was then mixed into about 15 ml of N-methyl-2-pyrrolidone for a minimum of one hour before two 10-minute sonication steps, after which the resulting slurry was further mixed on a hot plate at 100° C. for a minimum of 30 minutes before being sprayed onto a 10×10 cm, 10 μm thick aluminum foil heated to above 100° C. The foil was dried overnight in an oven at 70° C. in air before being punched with a biopsy punch. These punches were then used to make 2032 coin cells using lithium foil as anode, 1.0M LiPF650 / 50 ethylene carbonate / dimethyl carbonate solution as electrolyte, Celgard cell separator, 0.5 mm stainless steel spacer and a wave spring on the cathode side to ensure mechanical contact within the cell; each coin cell was assembled and sealed in a dry low oxygen argon atmosphere using a coin cell press.
[0112] Electrochemical Performance Studies The coin cells fabricated in the above process were subjected to potential limited galvanostatic testing with constant current using a low current Neware or bio-logic battery tester. The cells were cycled at rates ranging from C / 20 to C / 2 between 4.8 V and 2 V using constant current charge / discharge conditions.
[0113] For LRMO materials (Li x (Mn y Ni 1-y ) 2-x O2, wherein x=1.16, and y=0.7), Fig. 8A is a graph showing cell potential versus specific capacity, and Figure 8B is a plot of specific capacity versus cycling.
[0114] Reference Fig. 8A and 8B , it can be seen that the slowly cooled material has poor capacity and capacity retention. After 50 full charge / discharge (C / 2 rate) cycles, the material produced a specific capacity of 120 mAh / g at C / 20 rate, which is far below the theoretical performance of the material. In addition, there is significant voltage decay in the material, with the average discharge potential below 3 V after 30 cycles.
[0115] For an exemplary battery including a LRMO active material according to various embodiments of the present disclosure, Fig. 9A To show a graph of cell potential versus specific capacity during commissioning cycles of ultra-rapidly quenched materials, Fig. 9B is a graph showing cell potential versus specific capacity over time for an ultrafast quenched material, and Fig. 9C A graph showing specific capacity versus cycle at C / 20 rate for multiple cycles is shown. Fig.9D Long term cycling of an exemplary LRMO material shows that after 150 C / 5 cycles, the material exhibits less than 10% capacity fade in all three C / 20 reference cycles (which occur at cycles 56, 107, and 158).
[0116] and Figures 8A to 8B The exemplary LRMO cathode material produced using ultra-fast quenching performs well compared to the comparative exemplary materials shown. Figures 9A to 9C shown. Fig. 9A and 9BThe electrochemical performance data in demonstrate both that (a) highly functional materials can be produced on a meaningful scale, and (b) these materials have performance characteristics that meet or exceed much smaller batches produced. Notably, the voltage curve has an increased and desired inflection point after a discharge capacity of about 100 mAh / g compared to materials made using slower cooling methods. The voltage trajectory above this inflection point demonstrates that there is virtually no "sag" or loss during cycling, which is an improvement over materials made using slower transfer techniques. This suggests that ultra-fast cooling methods implemented using gravity-driven transfer from a furnace to a quench environment in 200 milliseconds are desirable when combined with precursors that rapidly decompose via microwave radiation.
[0117] Fig. 10A To show the LRMO active material (Li x (Mn y Ni 1-y ) 2-x A graph of cell potential versus specific capacity for a comparative cell having a cell potential of 0.02, wherein x=1.16, and y=0.7, Fig. 10B To show Fig. 10A A graph of the specific capacity of a battery versus the number of cycles, Fig. 10C To show the results for the first and 50th C / 2 discharge cycles, a water-quenched LRMO active material (Li x (Mn y Ni 1-y ) 2-x A graph of cell potential versus specific capacity for an exemplary cell having a capacitance of 0.02, wherein x=1.16, and y=0.7), and Fig. 10D To show Fig. 10C Specific capacity of the battery versus cycle number. The active material was not microwave treated.
[0118] Both the comparative cell and the exemplary cell were cycled twice with both the charge current and discharge current at a rate of about C / 20 to condition the cathode material. After this, 25 cycles were performed at a charge rate of C / 20 and a discharge rate of C / 2. This set of 27 cycles is referred to as one cycle, and all cells were subjected to this approach twice. Figures 10A to 10DAs can be seen, the rapidly quenched exemplary material has improved capacity and capacity retention relative to the capacity and capacity retention of the comparative material. After 50 full charge / discharge cycles, the exemplary material produced a specific capacity of nearly 230 mAh / g at a C / 2 rate, which is much better than the comparative material showing a much lower capacity and a lower average discharge voltage. Therefore, the exemplary material, a) shows a significant increase in capacity after 50 cycles, (b) does not show the excessive voltage decay commonly reported (where the average discharge voltage of the battery is significantly reduced after use), and (c) exceeds 250 mAh / g at a C / 20 discharge rate after 25 cycles, and exceeds 230 mAh (at a C / 2 rate) after 50 cycles, where the average voltage loss during discharge is less than 10%. After 50 full C / 20-C / 2 charge / discharge cycles, the specific capacity increased by 20% to 25%. In contrast, the comparative material has much lower performance, including a specific capacity value below 100 mAh / g.
[0119] Fig.11A To illustrate the various embodiments of the present disclosure, Li x (Mn y Ni 1-y ) 2-x A graph of cell potential versus specific capacity for an exemplary cell with O2 active material where x=1.16 and y=0.7, and Fig. 11B To show Fig.11A Specific discharge capacity versus cycle for an exemplary battery at C / 20 and C / 2 rates.
[0120] Therefore, if Figures 11A to 11B As shown, combining the microwave decomposition process with rapid thermal quenching produces a material that provides greater electrochemical stability. The combined microwave treatment and rapid quenching method caused a voltage drop that was greatly reduced compared to the voltage drop of the material of the comparative cell, and the discharge capacity was stable for about 200 cycles (at which time the coin cell test fixture used failed).
[0121] The synthesized LRMO active material (i.e., sintered and quenched loose powder) was mixed with Super-P carbon black and polyvinylidene fluoride (PVDF) in a ratio of 8:1.2:0.8, so that the active LRMO was 80% of the total mass. The resulting blend was then mixed into about 15 ml of N-methyl-2-pyrrolidone for a minimum of one hour. Two 10-minute sonication steps were then performed, after which the resulting slurry was further mixed on a hot plate at 100° C. for a minimum of 30 minutes and then sprayed onto a 10×10 cm, 10 μm thick aluminum foil heated to above 100° C. The foil was dried in an oven at 70° C. in air overnight before being sampled into a circular electrode disk. The resulting male mold was then used to make a 2032-size coin cell comprising a lithium foil anode, 1.0 M LiPF6 50 / 50 ethylene carbonate / dimethyl carbonate solution as electrolyte, Celgard cell separator, 0.5 mm stainless steel spacer, and a wave spring on the cathode side to ensure mechanical contact within the cell. Each coin cell was assembled and sealed in a dry low-oxygen argon atmosphere using a coin cell press.
[0122] The coin cells made in the above process were tested with a potential limited constant current using a LAND battery tester with a constant current. A minimum of three cells of each variant were cycled between 2.0V and 4.8V at ambient temperature. The cells were cycled twice with both the charge current and the discharge current at a rate of about C / 20 to condition the cathode material. The cells were then charged and discharged for 25 cycles at a C / 20 charge rate and a C / 2 discharge rate. These 27 cycles can be referred to as one cycle, and all cells were subjected to two cycles.
[0123] Fig. 12A To show the x = 0.25 sample (i.e. Li[Ni x Li( 1 / 3–2x / 3 )Mn (2 / 3-x / 3) ]O2 sample, where x = 0.25) during cycling, and Figures 12B to 12D Shown are the full charge and discharge curves of coin cells containing 25 Hq, 25 Lq and 25 Mq samples respectively. Fig.13A is a graph showing the specific discharge capacity of the x=0.17 sample during cycling, and Figures 13B to 13C Shown are the full charge and discharge curves of coin cells containing 17 Hq, 17 Lq and 17 Mq samples respectively. Fig.14A is a graph showing the specific discharge capacity of the x=0.10 sample during cycling, and Figures 14B to 14C Shown are the full charge and discharge curves of coin cells containing 10 Hq, 10 Lq and 10 Mq samples respectively.
[0124] Table III below shows the discharge capacity (DC) of the samples during cycling and the C / 20:C / 2 ratio of DC28 / DC27. Rate capability is evaluated by taking the ratio of the C / 20 discharge capacity to the C / 2 discharge capacity, e.g., the discharge capacity at the 27th and 28th cycles. Note that discharge cycles 1, 2, and 28 are at C / 20 rates, while discharge cycles 3, 27, and 54 are at C / 2 rates.
[0125] Table III
[0126]
[0127] Reference Figures 12A to 12C , the x=25 samples synthesized by different quenching methods exhibit different relative specific charge capacities in their first charge 4.5 V platform. Specifically, the platform of 25Hq accounts for 60.7% of the initial charge capacity, 25Lq accounts for 44.4%, and 25Mq accounts for only 34.5% of the capacity.
[0128] Among the samples with x = 0.25, the 25Hq has the highest initial capacity, which is 186 mAh g -1 , and 25Mq has the lowest initial capacity of 127mAh g -1 . As seen in Table III, all x=0.25 samples, except the 25Mq sample, see increased capacity during cycling. Of all three samples, the 25Hq sees the largest capacity increase. The 25Mq sample also shows severe voltage decay, with the voltage dropping to below 3V during cycling. Although the 25Hq and 25Lq samples also have an inflection point at 2.8V on their discharge curves, they do not show such severe voltage decay. No voltage decay is seen in the C / 20 discharge of the 25Hq and 25Lq samples, however the C / 20 discharge of the 25Mq sample experiences voltage decay. The average discharge voltage of the 0.25 samples reflects these voltage decays, with the 25Mq having the lowest average voltage during cycling, and the 25Lq having an average discharge voltage slightly higher than that of the 25Hq.
[0129] Regarding rate performance, as seen in Table III, the C / 20:C / 2 ratios for the 25Hq, 25Lq, and 25Mq samples are 1.19, 1.25, and 1.39, respectively.
[0130] Reference Figures 13A to 13D , the charging curve of the x = 0.17 sample has a more typical single flat 4.5 V platform at the first charge, which accounts for about 56.8% of the initial charge capacity, while the 17Lq and 17Mq samples show a less clear 4.5 V platform, which accounts for about 20% of the initial charge capacity in both cases.
[0131] Between the first two C / 20 discharges, the capacity of all x = 0.17 samples increased by about 10 mAh g -1 . As seen in Table III, the second C / 20 discharge sees a capacity increase of 31%, 73% and 91% for 17Hq, 17Lq and 17Mq respectively. There is an almost consistent voltage decay behavior for all three samples, and the average plateau voltage drops by about 0.4V during cycling. However, no voltage decay is seen in the C / 20 discharge curves for these samples. The x=0.17 sample also has a similar average discharge voltage over time. The main difference is how the average voltage of the 17Mq increases during the first cycle, but by the second cycle it matches the voltage decay trend of the 17Hq and 17Lq.
[0132] Reference Figures 14A to 14D , Regarding the charging curve of the x=0.10 sample, the 10Hq charging curve is different from that of the 10Lq and 10Mq samples, which have similar curves. Only the 10Hq sample has a clear 4.5V platform, although all three samples have a continuous inflection point at 4.5V, but the 10Hq disappears, while the 10Lq and 10Mq samples continue to the 54th cycle. The inflection point of the 10Mq sample is the most significant.
[0133] As can be seen in Table III, all x = 0.10 samples experienced approximately 5 mAh g during the first C / 20 cycle. -1 The initial capacity increases were followed by 300%, 60%, and 67% increases for the 10Hq, 10Lq, and 10Mq samples, respectively, during the second C / 20 discharge. By the end of the first C / 2 discharge, the capacities of all x=0.10 samples exceeded or caught up with the initial C / 20 capacity. During the two rounds of C / 2 discharge, 10Hq saw a capacity increase of 197% and 50%, 10Lq saw a capacity increase of 25% and 16%, and 10Mq saw an increase of 36% and 20%, respectively, during the first and second rounds. The discharge plateaus for the 10Lq and 10Mq samples started at about 3.0V, while the plateau for the 10Hq sample started at 3.2V; the voltage behavior of 10Hq during cycling was different from that of 10Lq and 10Mq. The voltage behavior of all x=0.10 samples was rate dependent, and the average discharge voltage of the C / 20 discharge for all three samples increased during cycling. However, the C / 2 discharge of the 10Lq and 10Mq samples showed signs of voltage decay, while that of the 10Hq did not.
[0134] In addition, the 10Lq and 10Mq samples have an inflection point at 2.2 V, which only exists on the C / 20 discharge curve. These voltage behaviors of the x=0.10 sample indicate that the average discharge voltage of the 10Lq and 10Mq samples is higher than that of 10Hq, but also show a greater degree of voltage decay.
[0135] Regarding rate performance, as shown in Table III, the C / 20:C / 2 ratios for the 10Hq, 10Lq, and 10Mq samples are 1.27, 1.60, and 1.67, respectively. It is worth noting that the effective charge and discharge per cycle also vary significantly with the cycle, making the DC28 / DC27 ratio of 10Hq actually a C / 10:C / 1 ratio.
[0136] The various phase changes during the testing are shown in the voltage curves observed during cycling. The expected voltage plateau seen in the x=0.25 sample indicates that the expected typical phase changes occurred.
[0137] Figures 15A to 15I Graph showing normalized and shifted XRD patterns of LRMO powder before and after cycling for 25Hq, 25Lq, 25Mq, 17Hq, 17Lq, 17Mq, 10Hq, 10Lq and 10Mq samples, respectively.
[0138] Reference Figures 15A to 15I After cycling, the XRD patterns of all x = 0.25 samples show that the 2θ = 22° superlattice peak disappears, indicating that there must be migration of transition metals to balance the structure. However, all other R-3m index peaks are retained, indicating that the overall structure is maintained. Similar results can be seen in the x = 0.17 and 10Hq samples. This loss of transition metal order is related to the loss of oxygen and lithium, and thus the capacity reduction, while Figures 12A to 14C The capacity increase seen in shows that this is not the case for these samples. Therefore, these data suggest that migration of transition metals does not always lead to capacity loss.
[0139] The 10Mq sample has a significantly different crystal structure after the cycle test, but both the 10Mq sample and the 10Lq sample still have some visible peaks at 22°, which further indicates that Figures 14A to 14C The electrochemical phase transition seen in Figures 12A to 13C The alternating phase transitions seen in 10Lq and 10Mq suggest that the synthetic limit of LRMO exists somewhere at a Ni content of 0.17>x>0.10.
[0140] Fig.16 Included are SEM micrographs at 50 k× of cathodes sprayed with 25Hq, 25Lq, and 25Mq samples before and after cycling. Fig.17Included are SEM micrographs at 50 k× of cathodes sprayed with 17Hq, 17Lq, and 17Mq samples before and after cycling. Fig.18 Included are SEM micrographs at 5k× of cathodes sprayed with 10Hq, 10Lq, and 10Mq samples before and after cycling.
[0141] Reference Figures 16 to 18 , in all samples with x=0.25 and x=0.17, Fig.16 and 17 The morphology of the as-fabricated and cycled cathodes seen in Figure 1 is uniform. Fig.18 The morphology of the x=0.10 sample seen in Figure 1 is inconsistent. 10Hq is consistent with the higher nickel content samples, while 10Lq and 10Mq are consistent with each other. All samples have consistent morphology before and after cycling; there is no evidence of changes in surface structure or particle morphology due to electrochemical cycling.
[0142] Both nickel content and quenching method affect the structure and electrochemical behavior of LRMO cathodes. In general, when synthesized with higher Ni content and / or faster quenching rate, the material has higher capacity and more typical voltage behavior, but the results are sometimes slightly different.
[0143] The XRD patterns of the LRMO powders show that the structure depends on both the nickel content and the quenching method. Slight crystallographic differences are expected between samples of different nickel contents and are observed between x=0.25 and x=0.17 and 10Hq samples. The XRD patterns of 10Lq and 10Mq have a large number of secondary peaks, while the XRD pattern of 10Hq does not. The secondary peaks seen in the patterns of 10Lq and 10Mq are consistent with the secondary peaks seen in the XRD patterns of 25Mq and 17Mq samples. These examples show that the quenching rate is important in determining the structure, phase content and phase purity.
[0144] The secondary lamellar phases found in many samples are likely the result of localized relative nickel-rich inhomogeneities with correspondingly larger lattice parameters. The (110) peak split is present in the XRD patterns of all samples except 25Hq and 25Lq, suggesting that the slower quenching results in nickel inhomogeneities. The XRD patterns of the 25Mq and 17Mq samples have additional secondary peaks at (101), (104), and (107) that are seen in the 10Lq and 10Mq samples. However, it must be noted that the (104) secondary peak of 25Mq and 10Lq may be due to contaminants. These additional peaks, while different, appear for all metal-quenched samples, suggesting how the structure depends on both nickel content and quenching. These data support the notion that, regardless of the Ni content, the slower quenching method produces separate nickel-rich phase regions, as well as the formation of contaminants in the material, which determines the local order of nickel in the sample. Fig.24 Schematic diagram showing the proposed structure of the secondary lamellar phase.
[0145] Because of Ni 2+ ions have a larger ionic radius than Mn ions, so it is believed that there is less local lattice expansion in the presence of less Ni. Samples with higher nickel content should have a higher degree of long-range order in the nickel ion distribution, and more favorable order produces a smaller lattice parameter. Rapid quenching of these samples maintains long-range order and a smaller lattice parameter, while slower quenching will allow contaminant nucleation and the development of nickel inhomogeneities, both of which will distort the average lattice parameter. Fig.26B The crossover point of the lattice parameter “a” seen in is at x=0.11, which further indicates that there is a synthetic limit of 0.17>x>0.10.
[0146] The electrochemical behavior of the samples is affected by both the nickel content and the quench method. The first charge behavior of the material is indicative of purity and capacity, as higher performing materials are known to exhibit a single strong plateau consistent with phase transitions caused by nickel-catalyzed oxygen and lithium losses.
[0147] Figures 19A to 19C Graph showing a smoothed spline fit of the dQ / dV vs. V data for the first charge cycle for the x=0.25, x=0.17, and x=0.10 samples.
[0148] Reference Figures 19A to 19C , the 4.5V peak seen on the dQ / dV plot indicates that all samples have an initial 4.5V plateau to some extent. Figures 12A to 14CIt shows that in the subsequent charge, only some samples have an inflection point at 4.5V. This shows that all samples initially experienced similar phase changes, but the persistence of the inflection point in some samples shows that the reaction is not always completed during the initial charge. The samples with secondary peaks in their spectra are the same as those with inflection points in the subsequent cycles, and therefore may be related. This is further supported by how the higher nickel content drives the secondary layered phase peak to the left of the main peak. Although some samples (such as 25Mq and 10Lq) show signs of rock salt contamination, the contamination does not rule out the possibility of some other phase changes. In any case, these transitions occur and gradually disappear during a large number of cycles, which shows that in the end, the sample is still completely and irreversibly transformed.
[0149] The presence of inflection points on the non-water quenched samples, in addition to some inflection points on 10Hq, provides further evidence that these inflection points are related to phase inhomogeneities. The 10Hq sample starts at these inflection points, but by the 54th cycle, its charge curve more closely resembles the x=0.17 sample than its initially similar x=0.10 sample. Therefore, these data are consistent with the development of nickel inhomogeneities that extend the 4.5V phase transition.
[0150] Figures 20A to 20C Graph showing a smoothed spline fit of the dQ / dV vs. V data for the second charge cycle for the x=0.25, x=0.17, and x=0.10 samples. Figures 21A to 21C is a graph showing the first C / 2 discharge and the last C / 2 discharge of the 25Hq, 25Lq and 25Mq samples, and Fig.21D Graph showing the average discharge voltage per cycle for the 25Hq, 25Lq and 25Mq samples during cycling. Figures 22A to 22C is a graph showing the first C / 2 discharge and the last C / 2 discharge of the 17Hq, 17Lq and 17Mq samples, and Fig.22D Graph showing the average discharge voltage per cycle for the 17Hq, 17Lq and 17Mq samples during cycling. Figures 23A to 23C is a graph showing the first C / 2 discharge and the last C / 2 discharge of the 10Hq, 10Lq and 10Mq samples, and Fig.23D Graph showing the average discharge voltage per cycle for the 10Hq, 10Lq and 10Mq samples during cycling.
[0151] The discharge curves of the samples also show that the cycling behavior over time is affected by the nickel composition and the quenching method. Figures 20A to 20C , the peaks of the water-quenched samples are initially lower in voltage than the LN2 and metal-quenched samples on average, indicating that nickel inhomogeneity affects the voltage. With the exception of 25Mq, the average discharge voltage of the water-quenched samples also tends to be lower than that of the other samples of the same composition. The dQ / dV patterns of 17Lq and 17Mq and Figures 21A to 23D The diagram shows how the discharge curves evolve different behaviors during cycling. The voltage of the x=0.17 sample, while the most uniform in terms of voltage behavior, also sees a greater degree of voltage decay. The exceptions to this are the 25Mq sample, which sees voltage decay during cycling; and the x=0.10 sample, which sees a voltage increase for its C / 20 discharge and a voltage decay for its C / 2 discharge. It is also important to note that the average voltage decay shown experienced by most of the samples is due to the greater capacity produced at these voltages, rather than degradation of the sample. The clear differences in discharge behavior seen in the samples suggest that differences in quench rates are also manifested in the different electrochemical reactions.
[0152] When compared to the voltage decay of the x = 0.17 sample, the voltage decay in 25Hq and 25Lq is smaller, and their associated voltage plateaus are also at different voltages. The smaller 25Hq and 25Lq voltage decays are mostly consistent with the phase transition to the spinel-like phase during cycling, which is associated with the 3V plateau. The more severe voltage decay of the x = 0.17 sample is also mostly consistent with the phase transition to the spinel-like phase. In both cases, but especially in the case of the x = 0.17 sample, the voltage plateau is close to the Ni in the manganese-rich environment. 2 + / 3+ / 4+ The average voltage of the redox phase indicates that these plateaus are driven by nickel redox and therefore nickel distribution. This voltage loss and nickel redistribution are mostly consistent with the evolution of the spinel-like phase, with the main inconsistency being the increase in capacity, which is related to both the increase and loss of initial capacity, and which seems to be generally related to significant structural degradation. Therefore, the voltage decay of the structurally robust 25Hq, 25Lq and x=0.17 samples may not be entirely due to the evolution of the spinel-like phase.
[0153] The evolution of a spinel-like phase also fails to explain the differences in behavior between discharge rates, particularly for the x=0.10 sample. The C / 20 discharge of the x=0.10 sample begins at a voltage similar to that of the decaying sample, and its voltage increases during cycling; the C / 2 discharge of the x=0.10 sample undergoes some degree of voltage decay. While the lower initial potentials of the samples may be related to their larger manganese concentrations and subsequent lower nickel redox potentials, the inconsistent voltage behavior cannot be fully attributed to the formation of a spinel-like phase, especially when considering their rapid capacity increase. In contrast, the lower manganese concentration, capacity loss, and faster voltage decay of 25Mq indicate the formation of a spinel-like phase. These factors (and indeed how its discharge voltage plateau starts at 3V) are consistent with a voltage decay mechanism for the evolution of a spinel-like phase. It is possible that phase impurities generated during slow quenching may make 25Mq more susceptible to the evolution of a spinel-like phase. The voltage plateau of 25Mq falls on the Mn 3+ / 4+The discharge plateaus of 10Lq and 10Mq are similar to those of 25Mq, starting at 3V, suggesting that these samples may also be undergoing some degree of transformation to a spinel-like phase. The XRD of all samples except 10Mq have peaks indicative of an R-3m layered structure, further suggesting that the evolution of the spinel-like phase is not entirely responsible for the voltage decay or capacity change.
[0154] Fig.24 Schematic diagram showing how phase impurity inclusions in a 25Mq sample with R-3m structure and lattice parameter a'>a give rise to secondary peaks as seen to the left of the 25Mq (104) peak. Fig.24 As shown, the redox of nickel driving the evolution of these plateaus indicates that the nickel content homogenizes over time.
[0155] The electrochemical cycling data for the LRMO cathodes see a continued increase in capacity, with the exception of the 25Mq. While the x=0.25 sample sees a slight increase in capacity, the x=0.17 sample sees a more significant increase, and the x=0.10 sample sees an even greater increase. Thus, regardless of the quenching method, the increase in specific capacity percentage during cycling exhibits an inverse relationship with nickel content. The largest capacity increase was seen in the 10Hq sample, followed by the 10Mq and 10Lq samples. Since impurities are associated with nickel inhomogeneities, this relationship suggests that the capacity increase is at least partially driven by homogenizing the nickel content during cycling due to the "electrochemical annealing" process.
[0156] Comparative XRD of the cycled cathode material with the original cathode material shows very similar behavior between all samples except 10Lq and 10Mq, where the transition metal superlattice peaks disappear after cycling. 10Lq has some retained superlattice peaks after cycling, and the 10Mq sample sees the appearance of several new peaks, marking a significant difference between the two samples. This difference further indicates the importance of the quench rate, as under slower quench conditions, there appears to be a synthetic lower limit for LRMO, where 0.17>x>0.10. However, the behavior of the 10Hq sample is different and shows that faster quenching of the sample can produce stability and long-term performance associated with higher Ni content samples.
[0157] Electrochemical testing of these materials showed that the rapidly quenched material had excellent capacity and capacity retention and was the only variant that showed an increase in capacity during cycling. After 50 full charge / discharge cycles, the material produced a specific capacity of nearly 230 mAh / g at a C / 2 rate, which is much better than the materials cooled in other ways.
[0158] It was found that such materials, using extremely rapid cooling by immersion in water during synthesis, produced materials with superior and differentiated crystal structures and electrochemical behaviors never before reported. Specifically, it was found that the water-quenched materials: (a) showed a significant increase in capacity over 50 cycles, (b) did not exhibit the commonly reported voltage decay (where the average discharge voltage of the battery decreases significantly after use), (c) had a specific capacity of over 250 mAh / g after 25 cycles at C / 2 rate and 4 cycles at C / 2 rate, and (d) had a specific capacity of over 230 mAh / g (e.g., 231 to 240 mAg / g) after 50 cycles at C / 2 rate, where the average voltage loss during discharge was less than 10% (e.g., as Fig.21D shown).
[0159] Fig.26A To show that the formula Li[Ni x Li (1 / 3–2x / 3) Mn (2 / 3-x / 3) ]O2 (where the nickel content x = 0.25) of the original LRMO active material powder. This formula can also be written as Li z (Mn y Ni 1-y ) 2-z O2, where z = 1.16, and y = 0.7, and formed using Hq, Lq, and Mq (ie, water quench, liquid nitrogen quench, and metal quench, respectively). Fig.26B Included are an upper graph showing the trend between the lattice parameter "a" and the nickel content of the sample obtained by single-phase Rietveld fitting, and a lower graph showing the trend between the lattice parameter "c" and the nickel content of the sample.
[0160] like Fig.26A As shown, X-ray diffraction evaluation of the materials showed that the materials had a hexagonal (e.g., rhombohedral) phase associated with LiNiO2 with a space group (R-3m) and a monoclinic phase associated with Li2NiO3 with a space group (C2 / c). This indicated that all samples had the expected layered structure. Notably, the monoclinic phase diffraction peak was the most clear in the samples produced by the Hq method, indicating that the method produced a more defined crystal structure.
[0161] There is also a superlattice peak near 22°, which is indicative of this family of compounds. The XRD patterns of the 10Lq and 10Mq samples also have significant peaks to the left of their (101), (104), (015), (107) and (108) peaks, indicating the presence of phase impurities with similar structure and larger lattice parameters than the bulk phase. The absence of other peaks indicates that in this case all impurities are isomorphous with the bulk of the material. The XRD pattern of the 10Hq sample shows only small additional (107), (108) and (110) peaks. Although the XRD patterns are not obvious, the 17Mq and 25Mq samples also have indications of phase impurities; there are small secondary peaks to the left of the (104) peak and its (107) peak, respectively. In addition, the (108) peak of the 25Mq sample has a shoulder to its left. A closer inspection of the (104) maximum shows that in the case of the secondary peaks of the 25Hq and 10Mq samples, the differences between the secondary peak groups indicate that the isostructural impurities may be nickel-rich layered structures, while the peaks of the 10Lq and 25Mq samples indicate that the isostructural impurities may be ordered rock salt. These data indicate that there should be two sources for these peak groups: one is an additional layered phase, and the other is contaminate rock salt. In this article, "secondary layered phase" will refer to local areas with compositional differences and corresponding structural deformations, specifically areas with higher nickel content and resulting larger lattice parameters, while "contaminate" refers to the rock salt phase.
[0162] Obtained using single-phase based Rietveld refinement Fig.26A The lattice parameters of the powders were 1.5 Å, ... Fig.26B It is shown that the lattice parameter "a" decreases with the nickel content in the sample regardless of the quenching technique. The same trend is also shown for the lattice parameter "c", but the x = 0.10, 0.17 and 0.25 samples quenched with liquid nitrogen deviate from this trend. The quenching method when x ≥ 0.10 shows that slower quenching methods may lead to larger lattice parameters "a". The overall trend of lattice parameter "c" is the same, except for 10Lq and 17Lq samples.
[0163] In one embodiment, a method of forming an active material for a positive electrode of a lithium-ion battery includes quenching a powder of the active material in water. In one embodiment, the method further includes firing the active material powder prior to quenching. The active material can be fired at a temperature of at least 800 °C. The water can be at room temperature prior to quenching, and the powder of the active material can be quenched at a rate of at least 1750 °C / second.
[0164] In one embodiment, the active material includes layered lithium-rich nickel manganese oxide. Excess Li, Ni, and Mn atoms can be uniformly and consistently distributed throughout the transition metal lattice sites such that there are no crystal volumes greater than 3×3×3 nm in which the ratios of Ni, Mn, and Li atoms differ from the average ratios of Ni, Mn, and Li atoms in the bulk material by more than 3%. The particles of the powder of the active material can be in the form of agglomerates having an average size range of from about 0.1 μm to about 20 μm, and the agglomerates of the powder of the active material are composed of microcrystals having an average size range of from about 25 nm to about 500 nm. The powder of the active material can contain a composite of a hexagonal phase and a monoclinic phase after quenching and is a combination of the LiMO2 R-3m phase and the Li2MnO3 C2 / m phase, where M is at least one of Ni or Mn. The powder of the active material can contain a solid solution having a crystal structure that predominantly or entirely possesses C2 / m symmetry. The powder of the active material can contain a solid solution having a crystal structure that predominantly or entirely possesses R-3m symmetry.
[0165] In one embodiment, the active material is represented by the formula Li[Ni x Li( 1 / 3–2x / 3 )Mn (2 / 3-x / 3) O2 (where 0 < x < 0.5). In one embodiment, the active material is substantially cobalt-free; and the active material is represented by the formula Li[Ni x Li( 1 / 3–2x / 3 )Mn (2 / 3-x / 3) O2 (where 0.19 < x < 0.26), or is represented by the formula Li[M x Li( 1 / 3–2x / 3 )Mn (2 / 3-x / 3) O2 (where 0.19 < x < 0.26, and where M includes at least one of Ti, Fe, Al, or Cr and Ni).
[0166] In one embodiment, the water comprises an additive solvated therein. The water may comprise 0.01 mol / L to 1.0 mol / L of the additive. In one embodiment, the additive comprises an acid which may be selected from the group consisting of sulfuric acid, citric acid, acetic acid, phosphoric acid, hydrochloric acid, ammonium phosphate, or a combination thereof. In another embodiment, the additive comprises a carbohydrate which may be selected from the group consisting of fructose, galactose glucose, lactose, maltose, sucrose, or a combination thereof.
[0167] In one embodiment, the active material is placed in the positive electrode of a lithium ion battery cell, which also includes a negative electrode and an electrolyte. Before electrochemical cycling of the battery, the active material comprises a hexagonal phase and a monoclinic phase; and after electrochemical cycling, the active material powder does not comprise a monoclinic phase.
[0168] In one embodiment, the specific discharge capacity of the battery cell increases by at least 10% after 50 electrochemical cycles at a charge rate of C / 20 and a discharge rate of C / 2 in the voltage range of 2V to 4.8V at room temperature, and the specific capacity of the battery cell is at least 230 mAh / g after 50 electrochemical cycles at a discharge rate of C / 2.
[0169] In one embodiment, a lithium-ion battery cell comprises: a negative electrode, an electrolyte, and a positive electrode, wherein the positive electrode comprises a layered lithium-rich nickel manganese oxide active material, wherein the specific discharge capacity of the battery cell increases by at least 10% after 50 electrochemical cycles at a charge rate of C / 20 and a discharge rate of C / 2, and after 50 electrochemical cycles at a discharge rate of C / 2, the battery cell has a specific capacity of at least 230 mAh / g.
[0170] In one embodiment, the specific discharge capacity of the battery cell increases by at least 10% at room temperature over a voltage range of 2V to 4.8V with a charge rate of C / 20 and a discharge rate of C / 20 for two electrochemical cycles, followed by a charge rate of C / 20 and a discharge rate of C / 2 for twenty-five electrochemical cycles, followed by a charge rate of C / 20 and a discharge rate of C / 2 for two additional electrochemical cycles, and then a charge rate of C / 20 and a discharge rate of C / 2 for twenty-five additional electrochemical cycles. In one embodiment, the average discharge voltage of the battery cell decreases by no more than 10% after 50 electrochemical cycles at a discharge rate of C / 2.
[0171] In one embodiment, the active material is of the formula Li[M x Li( 1 / 3–2x / 3 )Mn (2 / 3-x / 3)O2 (where 0 < x < 0.5, and M comprises Ni, or a combination of at least one of Ni, Al, Fe, or Cr and Ni). In one embodiment, the active material is substantially free of cobalt; and the active material is represented by the formula Li[M x Li (1 / 3–2x / 3) Mn (2 / 3-x / 3) O2 (where 0.19 < x < 0.26, and M comprises Ni). In one embodiment, the active material is represented by the formula y(LiMO2)·(1 - y)LiMnO3 (where y ranges from 0.8 to 1, and M comprises at least Ni and Mn).
[0172] In one embodiment, the particles of the active material powder are in the form of agglomerates having an average size range of about 0.1 μm to about 10 μm, and the agglomerates of the active material powder are composed of microcrystals having an average crystal size range of about 25 nm to about 500 nm; and the particles of the active material powder have at least one of a spinel surface layer, a carbon coating, or passivated oxygen bonds on the surface.
[0173] In one embodiment, excess Li, Ni, and Mn atoms are uniformly and homogeneously distributed throughout the transition metal lattice sites such that there is no crystal volume greater than 3 × 3 × 3 nm in which the ratio of Ni, Mn, and Li atoms differs from the average ratio of Ni, Mn, and Li atoms in the bulk material by more than 3%.
[0174] The foregoing description of the disclosed aspects is provided to enable any person skilled in the art to make or use the present invention. Various modifications to these aspects will be apparent to those skilled in the art, and the general principles defined herein can be applied to other aspects without departing from the scope of the present invention. Thus, the present invention is not intended to be limited to the aspects shown herein but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method, include: sintering the lithium rich metal oxide (LRMO) material at a sintering temperature to form a sintered LRMO material; as well as The sintered LRMO material is quenched from the sintering temperature to room temperature in less than 500 milliseconds to form a quenched LRMO material represented by the following chemical formula: Li x (Mr y Ni 1-y ) 2-x O 2 , Wherein x is greater than 1.05 and less than 1.25, and y ranges from 0.95 to 0.
1.
2. The method according to claim 1, in: The sintering temperature is at least 800° C.; and Rapidly cooling the sintered LRMO material from the sintering temperature to room temperature includes rapidly cooling the sintered LRMO material from the sintering temperature to room temperature in 200 milliseconds or less.
3. The method according to claim 1, in: The sintering temperature is 900° C. to 950° C.; and Rapidly cooling the sintered LRMO material from the sintering temperature to room temperature includes rapidly cooling the sintered LRMO material from the sintering temperature to room temperature within 100 milliseconds to 200 milliseconds.
4. The method according to claim 1, in: The sintering comprises sintering the LRMO material in a furnace; and Quenching the sintered LRMO material includes quenching the LRMO material in a quench bath.
5. The method according to claim 4, in: The time between removing the sintered LRMO material from the furnace and quenching the sintered LRMO material to room temperature of 25 degrees Celsius in the quench bath is 200 milliseconds or less; and The quench bath comprises an aqueous bath.
6. The method of claim 4, wherein the quench bath comprises a water bath, an alcohol bath, or an oil bath containing an additive, wherein the additive comprises an acid, a carbohydrate, an alcohol, or a combination thereof.
7. The method according to claim 1, further comprising: include: forming a mixture of water and metal organic precursors of lithium, nickel and manganese; heating the mixture to form a gel; as well as The gel is thermally decomposed using microwave radiation to form the LRMO material.
8. The method according to claim 7, in: The gel comprises a 0.01 to 0.20 mole fraction excess of the metal organic precursor of the lithium; and The LRMO material includes an inorganic LRMO material containing lithium, nickel, manganese, and oxygen.
9. The method of claim 1, further comprising drying the quenched LRMO material to form a LRMO active material, and providing the LRMO active material to a cathode electrode of a lithium ion battery comprising an anode electrode and an electrolyte.
10. The method of claim 9, wherein the LRMO active material exhibits at least one of the following: The crystalline particles of the LRMO active material exhibit a uniform distribution of Mn and Ni atoms throughout the crystalline particles such that when imaged by HAADF EDS, there are no Ni-rich or Mn-rich regions; The (006)+(102):(101) x-ray diffraction peak ratio increases by at least 6% compared to a non-quenched LRMO material having the same composition; The ratio of (003) to (104) x-ray diffraction peaks is greater than 2; Providing a specific capacity of at least 165 mAh / g upon first discharge of the lithium ion battery; After 200 charge / discharge cycles of the lithium ion battery, the average discharge voltage loss at a C / 20 rate is less than 10%; or The lithium-ion battery undergoes 200 C / 5 charge / discharge cycles with a capacity decay of less than 10%.
11. A method, include: thermally decomposing the precursor material using microwave radiation to form a thermally decomposed lithium-rich metal oxide (LRMO) material; sintering the thermally decomposed LRMO material to form a sintered LRMO material; as well as The sintered LRMO material is quenched to form a quenched LRMO material represented by the following chemical formula: Li x (Mr y Ni 1-y ) 2-x O 2 , Wherein x is greater than 1.05 and less than 1.25, and y ranges from 0.95 to 0.
1.
12. The method of claim 11, wherein the precursor material comprises a metal organic precursor of Li, Mn and Ni selected from at least one of acetates, carbonates, nitrates, sulfates or hydroxides of Li, Mn and Ni.
13. The method according to claim 12, further comprising: include: forming a mixture of water and said metal organic precursors of lithium, nickel and manganese; as well as The mixture is heated to form a gel, wherein the step of thermally decomposing the precursor material comprises heating the gel using the microwave radiation, and wherein the gel comprises the metal organic precursor in a 0.01 to 0.20 mole fraction excess of lithium.
14. The method of claim 11, wherein the precursor material comprises a precursor that is a co-precipitated hydroxide of Mn and Ni mixed with lithium carbonate.
15. The method of claim 11, wherein the quenching comprises quenching the sintered LRMO material from a sintering temperature to room temperature in less than 500 milliseconds to form a quenched LRMO material.
16. The method of claim 11, further comprising drying the quenched LRMO material to form a LRMO active material, and providing the LRMO active material to a cathode electrode of a lithium ion battery comprising an anode electrode and an electrolyte.
17. A cathode electrode active material represented by the following chemical formula: Li x (Mr y Ni 1-y ) 2-x O 2 , where x is greater than 1.05 and less than 1.25, and y ranges from 0.95 to 0.1, wherein the active material comprises a layered hexagonal phase and a monoclinic phase, and wherein the active material exhibits at least one of the following: (006)+(102):(101) X-ray diffraction peak intensity ratio is greater than 0.32 When included in a lithium-ion battery, provides a specific capacity of at least 165 mAh / g at a C / 20 rate during the first discharge; When included in the lithium-ion battery, after 100 charge / discharge cycles, the average discharge voltage loss at C / 20 rate is less than 10%; or When included in the lithium-ion battery, the capacity decay is less than 10% after 100 C / 5 charge / discharge cycles.
18. The active material of claim 17, wherein particles of the active material include a carbon coating or an acid-modified surface.
19. The active material of claim 17, wherein the active material exhibits the (106)+(102):(101) x-ray diffraction peak intensity ratio greater than 0.
32.
20. The active material of claim 19, wherein the active material exhibits a (003) to (104) x-ray diffraction peak ratio greater than 2.
21. The active material of claim 17, wherein the crystalline particles of the active material exhibit a uniform distribution of Mn and Ni atoms throughout the crystalline particles such that when imaged by HAADF EDS, there are no Ni-rich or Mn-rich regions.
22. A lithium ion battery, include: A cathode electrode comprising the active material according to claim 17; Anode electrode; and Electrolytes.
23. The battery of claim 22, wherein the active material provides a specific capacity of at least 165 mAh / g at a C / 20 rate upon first discharge of the lithium ion battery.
24. The battery of claim 22, wherein the lithium ion battery has an average discharge voltage loss of less than 10% at a C / 20 rate after 100 charge / discharge cycles.
25. The battery of claim 22, wherein the active material exhibits less than 10% capacity fade over 100 C / 5 charge / discharge cycles.
26. The battery according to claim 22, in: After 50 C / 20 (charging)-C / 2 (discharging) charge / discharge cycles, the average discharge voltage of the lithium-ion battery decreases by no more than 5%; or After 800 or more C / 20-C / 2 charge / discharge cycles, the discharge capacity of the lithium-ion battery is greater than 80% of its original capacity.
27. A method of operating a lithium ion battery according to claim 22, comprising performing a plurality of charge / discharge cycles, in: The active material provides a specific capacity of 165 mAh / g at a C / 20 rate during the first discharge of the lithium ion battery; After 100 charge / discharge cycles, the average discharge voltage loss of the lithium ion battery at a C / 20 rate is less than 10%; or The active material exhibited less than 10% capacity fade over 100 C / 5 charge / discharge cycles.