Hydrophilic anti-protein-adhesion hydrogel coating for medical catheter and preparation method and application of hydrophilic anti-protein-adhesion hydrogel coating

By applying organic hydrogel coatings prepared by copolymerizing polydopamine and functional polymers on medical catheters, the shortcomings of catheter materials in terms of biocompatibility, lubricity and antibacterial properties are solved, and efficient anti-protein adhesion and prevention are achieved. The performance of the dirty performance meets the high standards of modern medical care.

CN118873754APending Publication Date: 2024-11-01NANJING SHUANGWEI BIOTECH
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202410980717.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing medical catheter materials have shortcomings in biocompatibility, long-lasting lubricity, antibacteriality and anti-protein adhesion. Traditional surface modification technology is difficult to meet modern medical needs, especially the instability and biosafety of hydrophilic coatings. Problems are prominent.

Method used

Using a hydrophilic anti-protein adhesion hydrogel coating, including a polydopamine adhesion layer and an anti-fouling and anti-fungal organic hydrogel coating, through functional polymers, hydrophilic monomers, anti-fungal monomers and anti-fouling monomers The copolymerization reaction forms a semi-interpenetrating network structure, and the organic hydrogel layer is prepared in combination with the solvent replacement method to ensure the firmness and moisturizing properties of the coating.

Benefits of technology

The long-term hydrophilicity, antibacteriality and anti-protein adhesion of the catheter surface are achieved, which reduces the risk of infection, improves the patient's comfort, and meets different clinical application needs by adjusting the coating thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118873754A_ABST
    Figure CN118873754A_ABST
Patent Text Reader

Abstract

The invention relates to a medical catheter hydrophilic anti-protein adhesion hydrogel coating and a preparation method and application thereof, the prepared hydrogel coating surface coating has a two-layer structure, the inner layer is a polydopamine adhesion layer which can help the outer hydrogel layer to be firmly combined on the surface of a catheter; and the outer layer is an organic hydrogel layer and has antifouling, antibacterial, hydrophilic and moisturizing functions and the like. The hydrogel is of a semi-interpenetrating network structure and is tightly combined with the polydopamine layer through interaction mechanisms of ionic bonds, hydrogen bonds and the like, firm anchoring of the hydrophilic coating is ensured, the organic hydrogel layer is formed by copolymerizing a functional polymer, a hydrophilic monomer, an antifouling monomer and an antibacterial monomer to form the semi-interpenetrating network structure hydrogel, and the anti-fouling performance of the hydrogel is improved. The organic hydrogel layer is obtained through a solvent replacement method, non-specific adsorption of protein and various biological macromolecules on the surface of the catheter can be effectively blocked through zwitterions, and the risk of catheter-related infection is reduced. The antibacterial monomer can effectively kill common pathogenic bacteria such as escherichia coli and staphylococcus aureus. The functional polymer can improve the hydrophilicity of the hydrogel layer, and the viscosity of the solution and the thickness of the coating can be adjusted by changing the addition amount of the functional polymer, so that the possibility of coating customization is realized, and the requirements of different clinical application scenes are met. The preparation method disclosed by the invention is simple to operate, the coating is firm in combination, the biocompatibility is good, the lubricating property is excellent, and the coating can be applied to various biomedical catheters for transfusion, drainage, endoscopy and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomedical materials, and in particular to a hydrophilic protein-resistant hydrogel coating for a medical catheter and a preparation method and application thereof. Background Art

[0002] As a key medium connecting patients with treatment methods, the performance of medical catheters directly affects clinical effects and patient safety. With the diversification and complexity of medical needs, traditional materials and surface treatment technologies are difficult to meet the high standards of modern medical environments, including but not limited to biocompatibility, mechanical strength, antibacterial properties, and ease of operation. At present, medical catheters are mainly composed of hydrophobic polymers. The inherent low surface wettability of such materials not only increases the friction resistance during insertion, causing discomfort and even injury to patients, but also provides a breeding ground for bacterial adhesion, increasing the risk of postoperative infection. Traditional mitigation strategies, such as temporary application of lubricants, such as silicone oil, glycerol or lidocaine gel, can relieve friction in the short term. These lubrication methods have many problems, such as the lubricant is easy to fall off, the lubrication effect cannot be maintained for a long time, and it may even damage the urethra, and cause pathogenic microorganisms to multiply on the inner wall of the catheter, increasing the risk of urinary tract infection. Therefore, it is particularly urgent to develop medical coating materials with high biocompatibility, long-lasting superlubricity and effective antibacterial and anti-protein adhesion properties.

[0003] Existing surface modification technologies, such as chemical modification technologies, usually involve grafting hydrophilic monomers or polymer chains, such as polyethylene glycol (PEG) and polyvinyl pyrrolidone (PVP), onto the catheter surface to enhance surface wettability and reduce protein adhesion. However, chemical grafting methods are often limited by harsh reaction conditions, strong selectivity for substrates, and the possible introduction of harmful byproducts, which affect their wide applicability and biosafety. Physical modification technologies, including plasma treatment, corona discharge, and laser surface texturing, improve hydrophilicity and reduce friction by changing surface morphology or introducing polar groups. Although these methods can improve the initial wettability of the catheter to a certain extent, the instability of the modified layer and the possible damage to the bulk properties of the material during the treatment process limit their long-term effectiveness and reliability in clinical application. By adding nanoparticles (such as nanosilver, titanium dioxide) or bioactive molecules to the coating material in order to simultaneously obtain antibacterial and anti-protein adhesion, the stability and biosafety assessment of nanomaterials remains a major challenge. The method of adding antimicrobial agents has problems such as easy premature leakage and drug resistance. The catheter is modified with a hydrophilic coating. However, since the hydrophilic coating is not firmly bonded to the surface of the hydrophobic polymer material, the coating is easy to fall off, and the hydrophilic hydrogel layer is easy to lose water and dry, and has poor moisture retention, which affects the service life.

[0004] In summary, it is urgent to develop an innovative method for preparing medical catheter coatings with superior comprehensive performance to solve the problems of hydrophilicity, long-lasting lubricity, effective antibacterial properties and reduced protein adhesion in current medical catheters. Summary of the invention

[0005] In order to solve the deficiencies in the prior art, the present invention provides a hydrophilic anti-protein adhesion hydrogel coating for medical catheters and a preparation method and application thereof, which solve the problems of the current medical catheters in terms of hydrophilic properties, continuous lubrication performance, antibacterial efficacy and protein adhesion inhibition.

[0006] The technical solution adopted by the present invention is: a hydrophilic anti-protein adhesion hydrogel coating, which includes a polydopamine adhesion layer and an antifouling and antibacterial organic hydrogel coating from bottom to top. The antifouling and antibacterial organic hydrogel coating is obtained by polymerizing a functional polymer, a hydrophilic monomer, an antibacterial monomer, and an antifouling monomer to obtain a hydrogel, and part of the water molecules in the hydrogel are replaced by organic molecules to form an organic hydrogel coating.

[0007] Specifically, the functional polymer is polyvinyl pyrrolidone (PVP).

[0008] Specifically, the hydrophilic monomer is one or more of acrylic acid, methacrylic acid and acrylamide.

[0009] Specifically, the antifouling monomer is one or more of carboxylic acid betaine methyl methacrylate (CBMA), 2-methacryloyloxyethyl phosphorylcholine (MPC), and methacryloylethyl sulfobetaine (SBMA).

[0010] Specifically, the antibacterial monomer is methacryloyloxyethyl trimethylammonium chloride (DMC).

[0011] A method for preparing a hydrophilic protein-resistant hydrogel coating comprises the following steps: (1) Preparation of polydopamine (PDA) adhesion layer: prepare a dopamine reaction solution containing dopamine hydrochloride, tris(hydroxymethyl)aminomethane) and water, adjust the pH to 8-10, immerse the catheter in the prepared solution and react at room temperature for 12-48 hours under shaking. Dopamine will self-polymerize on the surface of the catheter. After taking it out, rinse it with deionized water, so that the surface of the catheter is covered with a layer of polydopamine adhesion layer; (2) Preparation of antifouling and antibacterial organic hydrogel coating: preparing an aqueous solution containing a functional polymer, a hydrophilic monomer, an antibacterial monomer, an antifouling monomer, a crosslinking agent, a thermal initiator and an accelerator, immersing a catheter with a polydopamine coating on its surface into the mixed solution for 30-60 minutes, pulling it out, and then thermally curing it for 1-10 hours, thereby forming a semi-interpenetrating network hydrogel coating on the surface of the catheter, wherein the mass ratio of the hydrophilic monomer, the antibacterial monomer, the antifouling monomer and the functional polymer is 100:5:5:0.1-100:50:50:10, preferably 100:10:10:0.2-100:30:30:5, the mass ratio of the crosslinking agent to the monomer is 0.1%-1%, the mass ratio of the thermal initiator to the monomer is 0.05%-2%, and the mass ratio of the accelerator to the monomer is 0.05-2%; (3) Hydration: Immerse the catheter obtained in the above step in deionized water for 6-24 hours to allow the hydrogel layer to fully swell and remove unreacted monomers; (4) Solvent replacement: The catheter obtained in the above step is immersed in an organic solvent for 0.5-4 hours to perform solvent replacement, thereby partially replacing the water molecules in the hydrogel layer with organic molecules to form an organic hydrogel layer-coated catheter.

[0012] Specifically, in the step (1), the molar ratio of dopamine hydrochloride to tris(hydroxymethyl)aminomethane is 1:1 to 1:10.

[0013] Specifically, in the step (1), the concentration of tris(hydroxymethyl)aminomethane in water is 30-100 mM.

[0014] Specifically, in the step (1), the dopamine concentration of the dopamine reaction solution is 1-5 mg / mL.

[0015] Specifically, in step (2), the functional polymer is polyvinyl pyrrolidone (PVP).

[0016] Specifically, in the step (2), the hydrophilic monomer is one or a mixture of two of acrylic acid, methacrylic acid, and acrylamide.

[0017] Specifically, in the step (2), the antifouling monomer is one of carboxylic acid betaine methyl methacrylate (CBMA), 2-methacryloyloxyethyl phosphorylcholine (MPC), and methacryloylethyl sulfobetaine (SBMA).

[0018] Specifically, in the step (2), the antibacterial monomer is methacryloyloxyethyltrimethylammonium chloride (DMC).

[0019] Specifically, the promoter in step (2) is tetramethylethylenediamine (TEMED).

[0020] Specifically, the initiator in step (2) is a thermal initiator, a peroxide initiator or an azo compound initiator, preferably a thermal initiator potassium persulfate.

[0021] Specifically, in the step (2), the crosslinking agent is selected from any one of N,N-methylenebisacrylamide, 1,5-hexadiene, ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, ethylene glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol diacrylate, glycerol trimethacrylate, glycerol triacrylate, glycerol dimethacrylate, and glycerol diacrylate. N,N-methylenebisacrylamide is preferred.

[0022] Specifically, in step (4), the organic solvent is a single solvent or a mixed solvent of multiple solvents such as glycerol, ethylene glycol, hexylene glycol, sorbitol, etc.

[0023] The invention discloses an application of a hydrophilic protein-resistant hydrogel coating in preparing a surface coating material for a medical catheter.

[0024] The beneficial effects of the present invention are as follows: the present invention provides a hydrophilic anti-protein adhesion hydrogel coating for medical catheters and a preparation method and application thereof, which have the following advantages: (1) The gel coating surface coating of the present invention has a two-layer structure, the inner layer is a polydopamine adhesion layer, which can help the outer hydrogel layer to firmly bond to the catheter surface; the outer layer is an organic hydrogel layer, which provides antifouling, antibacterial, hydrophilic, moisturizing and other functions. The hydrogel is a semi-interpenetrating network structure, which is tightly combined with the polydopamine layer through interaction mechanisms such as ionic bonds and hydrogen bonds, ensuring the firm anchoring of the hydrophilic coating.

[0025] (2) The organic hydrogel layer is formed by copolymerization of functional polymers, hydrophilic monomers, antifouling monomers and antibacterial monomers to form a semi-interpenetrating network structure hydrogel, and then the organic hydrogel layer is obtained by solvent replacement method. The monomers can form a semi-interpenetrating network structure with the functional polymers through polymerization reaction, thereby improving the mechanical properties of the hydrogel. Zwitterions can effectively block the nonspecific adsorption of proteins and various biomacromolecules on the catheter surface, reducing the risk of catheter-related infection. Antibacterial monomers can effectively kill common pathogens such as Escherichia coli and Staphylococcus aureus. Functional polymers can improve the hydrophilicity of the hydrogel layer, and by changing the amount of addition, the viscosity of the solution can be adjusted, the thickness of the coating can be changed, and the possibility of customized coating can be realized to meet the needs of different clinical application scenarios.

[0026] (3) Part of the water in the hydrogel layer is replaced with an organic solvent to prepare an organic hydrogel. On the one hand, the hydrogel generated by copolymerization of hydrophilic monomers, zwitterionic monomers and antibacterial monomers can form a large number of hydrogen bonds between molecular chains, which is conducive to the formation of a hydration layer, giving the catheter surface excellent hydrophilic properties and reducing friction resistance. However, a large amount of water is easy to evaporate, and the coating has poor moisture retention. After part of the water is replaced with organic solvents such as glycerol and ethylene glycol, there are strong hydrogen bond interactions between these organic solvents and the hydrogel and water molecules, and the boiling point of organic solvents such as glycerol and ethylene glycol is higher than that of water, thereby improving the moisturizing effect of the hydrogel layer, and is more conducive to improving the lubricity of the catheter and optimizing the patient's comfort.

[0027] (4) The preparation method of the present invention is simple to operate, the coating has firm bonding, good biocompatibility, and excellent lubrication performance, and can be applied to a variety of biomedical catheters such as infusion, drainage, and endoscopy. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the infrared spectrum of the coating-modified catheter prepared in Example 2 of the present invention.

[0029] Figure 2 The scanning electron microscope characterization images of the coating modified catheter prepared in Example 5 of the present invention; (a) catheter surface; (b) catheter cross section Figure 3 Graphs showing water contact angles of the coating-modified catheters of Examples 1-4 of the present invention.

[0030] Figure 4 1 is a comparison chart of the adsorption of BSA protein by the coating-modified catheters of Examples 1-4 of the present invention; (a) BSA protein concentration 0.5 mg / mL; (b) BSA protein concentration 1.0 mg / mL.

[0031] Figure 5 It is a stability test diagram of the coating modified catheter of Examples 1-4 of the present invention.

[0032] Figure 6 It is a moisture retention curve diagram of the hydrogel and organogel prepared in Example 4 of the present invention. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Example 1: Preparation of hydrophilic coating for medical catheters.

[0035] Step 1: Add tris(hydroxymethyl)aminomethane (3.03 g) and 500 mL of deionized water to a beaker, disperse them evenly by ultrasonication, then add glacial acetic acid dropwise to the solution, and use a pH meter to measure the pH value until the desired pH value (8.5) is reached. Weigh 0.1 g of dopamine hydrochloride and 50 mL of tris(hydroxymethyl)aminomethane buffer solution to a beaker, disperse them evenly by ultrasonication, then soak the cut clean medical catheter in the solution, place the beaker in a magnetic stirrer and stir at room temperature for 24 h, rinse with deionized water after stirring, and a medical catheter coated with PDA can be obtained.

[0036] Step 2: Weigh 0.3 g [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonatepropyl)ammonium hydroxide (SBMA), 1.2 g acrylic acid (AA), 0.2 g methacryloyloxyethyl trimethylammonium chloride (DMC), 0.0017 g N,N'methylenebisacrylamide (MBA), 0.012 g potassium persulfate (KPS), 5 μL tetramethylethylenediamine (TEMED), 0.01 g polyvinylpyrrolidone (PVP) and 2 mL deionized water into a beaker, and ultrasonicate the solution for 20 minutes at room temperature to fully mix and form a homogeneous solution. Soak the catheter with a layer of polydopamine coating on the surface in the hydrophilic hydrogel solution for 45 minutes so that the surface of the medical catheter is evenly coated with a layer of hydrogel solution, and then put it into an electric constant temperature blast drying oven and heat it at 60°C for 4 hours. After taking it out, the surface of the medical catheter can be coated with a layer of hydrogel coating.

[0037] Step 3: The catheter with the hydrogel coating formed on the surface was immersed in deionized water for 12 hours, so that the hydrogel layer was fully swollen and the unreacted monomers were removed.

[0038] Step 4: The catheter in step 3 was immersed in glycerol for 3 hours to obtain an organohydrogel-coated catheter.

[0039] Example 2: Preparation of hydrophilic coating for medical catheters.

[0040] Step 1 is the same as that in Example 1.

[0041] Step 2: Weigh 0.3 g [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonic acid propyl) ammonium hydroxide (SBMA), 1.2 g acrylic acid (AA), 0.2 g methacryloyloxyethyl trimethyl ammonium chloride (DMC), 0.0017 g NN methylenebisacrylamide (MBA), 0.012 g potassium persulfate (KPS), 5 μL tetramethylethylenediamine (TEMED), 0.02 g polyvinylpyrrolidone (PVP) and 2 mL deionized water into a beaker, and ultrasonicate the solution for 20 minutes at room temperature to fully mix and form a homogeneous solution. Soak the catheter with a layer of polydopamine coating on the surface in the hydrophilic hydrogel solution for 45 minutes so that the surface of the medical catheter is evenly coated with a layer of hydrogel solution, and then put it into an electric constant temperature blast drying oven and heat it at 60°C for 4 hours. After taking it out, the surface of the medical catheter can be coated with a layer of hydrogel coating.

[0042] Step 3: Same steps as in Example 1.

[0043] Step 4: Same steps as in Example 1.

[0044] Example 3: Preparation of hydrophilic coating for medical catheters.

[0045] Step 1 is the same as that in Example 1.

[0046] Step 2: Weigh 0.3 g [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonatepropyl)ammonium hydroxide (SBMA), 1.2 g acrylic acid (AA), 0.2 g methacryloyloxyethyl trimethylammonium chloride (DMC), 0.0017 g NN methylenebisacrylamide (MBA), 0.012 g potassium persulfate (KPS), 5 μL tetramethylethylenediamine (TEMED), 0.03 g polyvinylpyrrolidone (PVP) and 2 mL deionized water into a beaker, and ultrasonicate the solution for 20 minutes at room temperature to mix it thoroughly and form a homogeneous solution. Soak the catheter with a layer of polydopamine coating on the surface in the hydrophilic hydrogel solution for 45 minutes so that the surface of the medical catheter is evenly coated with a layer of hydrogel solution, and then put it into an electric constant temperature blast drying oven and heat it at 60°C for 4 hours. After taking it out, the surface of the medical catheter can be coated with a layer of hydrogel coating.

[0047] Step 3: Same steps as in Example 1.

[0048] Step 4: Same steps as in Example 1.

[0049] Example 4: Preparation of hydrophilic coating for medical catheters.

[0050] Step 1 is the same as that in Example 1.

[0051] Step 2: Weigh 0.3 g [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonatepropyl)ammonium hydroxide (SBMA), 1.2 g acrylic acid (AA), 0.2 g methacryloyloxyethyl trimethylammonium chloride (DMC), 0.0017 g NN methylenebisacrylamide (MBA), 0.012 g potassium persulfate (KPS), 5 μL tetramethylethylenediamine (TEMED), 0.04 g polyvinylpyrrolidone (PVP) and 2 mL deionized water into a beaker, and ultrasonicate the solution for 20 minutes at room temperature to fully mix and form a homogeneous solution. Soak the catheter with a layer of polydopamine coating on the surface in the hydrophilic hydrogel solution for 45 minutes so that the surface of the medical catheter is evenly coated with a layer of hydrogel solution, and then put it into an electric constant temperature blast drying oven and heat it at 60°C for 4 hours. After taking it out, the surface of the medical catheter can be coated with a layer of hydrogel coating.

[0052] Step 3: Same steps as in Example 1.

[0053] Step 4: Same steps as in Example 1.

[0054] Example 5: Preparation of hydrophilic coating for medical catheters.

[0055] Step 1 is the same as that in Example 1.

[0056] Step 2: Weigh 0.3 g 2-methacryloyloxyethyl phosphorylcholine (MPC), 1.2 g methacrylic acid, 0.2 g methacryloyloxyethyl trimethylammonium chloride (DMC), 0.0017 g ethylene glycol dimethacrylate, 0.012 g ammonium persulfate, 8 μL tetramethylethylenediamine (TEMED), 0.1 g polyvinylpyrrolidone (PVP) and 2 mL of deionized water into a beaker, and ultrasonicate the solution for 20 minutes at room temperature to fully mix and form a homogeneous solution. Soak the catheter with a layer of polydopamine coating on the surface in the hydrophilic hydrogel solution for 45 minutes so that the surface of the medical catheter is evenly coated with a layer of hydrogel solution, and then put it into an electric constant temperature blast drying oven and heated at 40°C for 6 hours. After taking it out, the surface of the medical catheter can be coated with a layer of hydrogel coating.

[0057] Step 3: The catheter with the hydrogel coating formed on the surface was immersed in deionized water for 18 hours to allow the hydrogel layer to swell fully and remove unreacted monomers.

[0058] Step 4: The treated catheter was immersed in a glycerol and ethylene glycol (1:1) solution for 3 h to obtain an organohydrogel-coated catheter.

[0059] Example 6: Preparation of hydrophilic coating for medical catheters.

[0060] Step 1: Tris(hydroxymethyl)aminomethane (3.03 g) and 500 mL of deionized water were added to a beaker and dispersed evenly by ultrasonication. Then, glacial acetic acid was added dropwise to the solution and the pH value was measured by a pH meter until the desired pH value (9) was reached. 0.1 g of dopamine hydrochloride and 50 mL of tris(hydroxymethyl)aminomethane buffer were weighed and added to a beaker and dispersed evenly by ultrasonication. Then, the clean cut medical catheter was immersed in the solution and the beaker was placed in a magnetic stirrer and stirred at room temperature for 36 h. After stirring, it was rinsed with deionized water to obtain a medical catheter coated with PDA.

[0061] Step 2: 0.3 g carboxylic acid betaine methyl methacrylate, 1.2 g acrylamide, 0.2 g methacryloyloxyethyl trimethyl ammonium chloride (DMC), 0.0017 g triacrylate glycerol, 0.012 g ammonium persulfate, 5 μL tetramethylethylenediamine (TEMED), 0.02 g polyvinyl pyrrolidone (PVP) and 2 mL deionized water were weighed and added to a beaker, and the solution was ultrasonicated for 20 minutes at room temperature to fully mix and form a homogeneous solution. The catheter with a layer of polydopamine coating on the surface was immersed in the hydrophilic hydrogel solution for 45 minutes, so that the surface of the medical catheter was evenly coated with a layer of hydrogel solution, and then placed in an electric constant temperature blast drying oven and heated at 30°C for 8 hours. After taking out, the surface of the medical catheter can be coated with a layer of hydrogel coating.

[0062] Step 3: The catheter with the hydrogel coating formed on the surface was immersed in deionized water for 8 hours to allow the hydrogel layer to swell fully and remove unreacted monomers.

[0063] Step 4: The treated catheter was immersed in hexylene glycol for 2 hours to obtain an organohydrogel-coated catheter.

[0064] Comparative Example 1: The PVC tube was cleaned with ethanol and deionized water without subsequent hydrophilic modification.

[0065] Characterization 1: Infrared spectrum test of medical catheters The modified medical catheter samples were analyzed by infrared spectroscopy using an FTIR-85 infrared spectrometer. The sample was placed directly between the crystal and the ejector pin of the ATR accessory, ensuring that the flatter side was in close contact with the ATR crystal surface. The pressure rod that fixed the sample was gently tightened to ensure that the sample was in close contact with the crystal. The Fourier transform infrared spectrometer was turned on and the spectral range of the spectrometer was set to 400-4000 cm -1 , and scanned 32 times, the infrared spectrum of the sample in Example 2 is as follows Figure 1 As shown. 2950 cm -1 and 2870 cm -1 The peak at 1250 cm-1 is attributed to the stretching vibration of the CH bond. These absorption peaks are mainly from the stretching vibration of the methylene group in acrylic acid and SBMA. -1 The peak at corresponds to the stretching vibration of the COC bond and the stretching vibration of the methacryloyloxyethyl group in DMC. These characteristic peaks prove that the medical catheter has been successfully coated with the hydrogel coating.

[0066] Characterization 2: Scanning electron microscopy test of medical catheters Su8010 SEM was used to observe the microscopic morphology of the surface of the medical catheter coated with the hydrogel coating. The medical catheter sample was placed in a vacuum drying oven and subjected to SEM examination after drying. Figure 2 As shown in the image, it can be seen that the surface presents an uneven morphology with multiple particles and holes of different sizes distributed in it. These particles represent the polymer network structure of the hydrogel, while the holes reflect the voids inside the material or the tiny defects formed when it combines with the substrate. The cross-section of the catheter presents a multi-layer structure, including the bottom material, the middle polydopamine coating, and the outermost layer of hydrogel. The bottom material looks relatively smooth and is the main part of the catheter. The middle polydopamine coating appears as a thin and uneven film, which acts as an adhesive to firmly attach the organic hydrogel layer to the catheter. The outermost organic hydrogel layer presents a porous structure with a thickness of about 80 μm.

[0067] Characterization 3: Medical catheter surface wettability test The contact angles of the reference original PVC tube and the modified medical catheter were measured using a contact angle meter DSA 25 to characterize the surface wettability of the medical catheter. The moisture on the catheter surface was wiped dry, and the sample was flattened on a glass slide. 2 μL of deionized water was added to the surface. Three groups of contact angle photos were collected and the average value was taken. The surface wettability of the medical catheter was as follows: Figure 3As shown. Compared with the water contact angles of the medical catheters of Comparative Example 1, Example 1, Example 2, Example 3, and Example 4, for Comparative Example 1, the water contact angle of pure PVC is 82.3°, indicating that it is hydrophobic. For Example 1, the water contact angle is 64.8°, indicating that the presence of the hydrogel coating enhances the hydrophilicity of the material. With the increase of PVP content, the water contact angle further decreases to 56.5°, 53.2°, and 37.8°, indicating that the introduction of PVP further improves the hydrophilicity of the hydrogel coating.

[0068] Characterization 4: Anti-bovine serum albumin (BSA) adsorption test for medical catheters The reference original PVC tube, the medical catheters prepared in Example 1, Example 2, Example 3, and Example 4 were immersed in an aqueous solution containing FITC-labeled bovine serum albumin (0.4 mg / mL) for 24 h. The samples were cultured in a constant temperature shaker at 37°C with a rotation speed of 100 rpm for 24 h. Subsequently, the supernatant was taken, the absorbance was measured, and the protein concentration and protein amount adsorbed by the sample were calculated according to the standard curve.

[0069] Depend on Figure 4 The protein adsorption rate of comparative example 1 at 0.5 mg / mL BSA concentration is 127 μg / cm 2 The protein adsorption rates of Example 1, Example 2, Example 3 and Example 4 were 110, 98, 78 and 52 μg / cm 2 The protein adsorption rate of comparative example 1 at 1 mg / mL BSA concentration was 1345 μg / cm 2 The protein adsorption rates of Example 1, Example 2, Example 3 and Example 4 were 916, 630, 379 and 117 μg / cm 2 .Depend on Figure 4 It can be concluded that the surface-modified medical catheters can better resist BSA adsorption, and with the increase of PVP content, the anti-protein adhesion ability of the catheter surface gradually increases.

[0070] Characterization 5: Medical catheter coating stability test The medical catheters prepared in Example 1, Example 2, Example 3, and Example 4 were placed in flowing PBS for 14 days, and the surface contact angle of the medical catheters was measured using a contact angle meter DSA 25 to characterize the coating stability of the medical catheters. The moisture on the surface of the catheter was wiped dry, and the sample was flattened on a glass slide. 2 μL of deionized water was dripped on the surface, and 3 groups of contact angle photos were collected and the average value was taken. Stability test of medical catheter coated with hydrophilic coating is as follows Figure 5For the medical catheters prepared in Example 1, Example 2, Example 3, and Example 4, the water contact angle after 14 days has no significant change compared with that before 14 days, indicating that the modified medical catheter coating has strong adhesion and stability, and the coating is not easy to fall off.

[0071] Characterization 6: Moisture retention performance test of hydrogel coating According to the method of step 2 in Example 4, two groups of hydrogels were prepared and named as hydrogels. Subsequently, one of the hydrogels was immersed in glycerol for 3 hours and named as organic hydrogel. The initial weight was weighed and then placed in a 37 degree constant temperature box. The weight was weighed at regular intervals and the moisture retention rate at each time was calculated. The moisture retention performance of the hydrogel and the organic hydrogel was compared. Figure 6 As shown in the figure, the water loss rate of the hydrogel is significantly higher than that of the organic hydrogel. The moisture retention rate of the hydrogel after 24 hours is 46%, while that of the organic hydrogel after 24 hours is 87%. It can be seen that the organic hydrogel prepared by the solvent replacement method can greatly improve the moisture retention performance.

[0072] The above are only preferred embodiments of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should be regarded as the protection scope of the present invention.

[0073] Technical personnel should note that although the present invention has been described according to the above specific implementation methods, the inventive concept of the present invention is not limited to this invention, and any modification using the inventive concept will be included in the scope of protection of this patent.

Claims

1. A hydrophilic anti-protein adhesion hydrogel coating, characterized in that: The hydrophilic anti-protein adhesion hydrogel coating comprises a polydopamine adhesion layer and an antifouling and antibacterial organic hydrogel coating from bottom to top. The antifouling and antibacterial organic hydrogel coating is composed of a functional polymer, a hydrophilic monomer, an antibacterial monomer, and an antifouling monomer. The water molecules in the antifouling and antibacterial organic hydrogel coating undergo solvent replacement, and part of the water molecules are replaced by organic molecules to form an organic hydrogel coating.

2. A hydrophilic protein-resistant hydrogel coating according to claim 1, characterized in that: The functional polymer is polyvinyl pyrrolidone (PVP).

3. The hydrophilic anti-protein adhesion hydrogel coating according to claim 1, characterized in that: The hydrophilic monomer is one or more of acrylic acid, methacrylic acid and acrylamide.

4. The hydrophilic anti-protein adhesion hydrogel coating according to claim 1, characterized in that: The antifouling monomer is one or more of carboxylic acid betaine methyl methacrylate (CBMA), 2-methacryloyloxyethyl phosphorylcholine (MPC), and methacryloylethyl sulfobetaine (SBMA).

5. The hydrophilic anti-protein adhesion hydrogel coating according to claim 1, characterized in that: The antibacterial monomer is methacryloyloxyethyl trimethylammonium chloride (DMC).

6. A method for preparing the hydrophilic protein-resistant hydrogel coating according to claim 1, characterized in that: The following steps are involved: (1) Preparation of polydopamine (PDA) adhesion layer: prepare a dopamine reaction solution containing dopamine hydrochloride, tris(hydroxymethyl)aminomethane) and water, adjust the pH to 8-10, immerse the catheter in the prepared solution and react at room temperature for 12-48 hours under shaking. Dopamine will self-polymerize on the surface of the catheter. After taking it out, rinse it with deionized water, so that the surface of the catheter is covered with a layer of polydopamine adhesion layer; (2) Preparation of antifouling and antibacterial organic hydrogel coating: preparing an aqueous solution containing a functional polymer, a hydrophilic monomer, an antibacterial monomer, an antifouling monomer, a crosslinking agent, a thermal initiator and an accelerator, immersing a catheter with a polydopamine coating on its surface into the mixed solution for 30-60 minutes, pulling it out, and then thermally curing it for 1-10 hours to form a semi-interpenetrating network hydrogel coating on the surface of the catheter, wherein the mass ratio of the hydrophilic monomer, the antibacterial monomer, the antifouling monomer and the functional polymer is 100:5:5:0.1-100:50:50:10; (3) Hydration: Immerse the catheter obtained in the above step in deionized water for 6-24 hours to allow the hydrogel layer to fully swell and remove unreacted monomers; (4) Solvent replacement: The catheter obtained in the above step is immersed in an organic solvent for 0.5-4 hours to perform solvent replacement, thereby partially replacing the water molecules in the hydrogel layer with organic molecules to form an organic hydrogel layer-coated catheter.

7. The preparation method according to claim 6, characterized in that: In the step (1), the molar ratio of dopamine hydrochloride to tris(hydroxymethyl)aminomethane is 1:1 to 1:

10.

8. The preparation method according to claim 6, characterized in that: The accelerator in step (2) is tetramethylethylenediamine (TEMED).

9. The preparation method according to claim 6, characterized in that: The initiator in step (2) is a thermal initiator, a peroxide initiator or an azo compound initiator.

10. Use of the hydrophilic anti-protein adhesion hydrogel coating according to claim 1 in preparing a surface coating material for a medical catheter.

Citation Information

Cited By

  • Antibacterial and anti-cell adhesion urinary system drainage tube as well as preparation method and application thereof

    CN120114662A

  • Toughening film composite fabric and preparation method thereof

    CN120273192A

  • Tracheal catheter with antibacterial and lubricating functions and preparation method thereof

    CN120514932A

  • Tracheal tube with antibacterial lubricating function and preparation method thereof

    CN120514932B

  • Urinary catheter and preparation method thereof

    CN120837739A