Large-area gas separation membrane and preparation method thereof
Through the modification of fillers and nanocomposite fillers in the preparation method, the problem of insufficient carbon dioxide transmission path of the existing gas separation membrane under large size and ultra-thin conditions is solved, and the carbon dioxide permeability coefficient and selectivity of the gas separation membrane are improved, thus achieving more Efficient gas separation performance.
Patent Information
- Application Number
- CN202410929113.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-11
AI Technical Summary
When existing gas separation membranes meet large-size and ultra-thin conditions, it is difficult to build an effective transmission path for carbon dioxide, resulting in poor carbon capture effect.
Using a large-area gas separation membrane preparation method, zinc nitrate reacts with sodium hydroxide to form a zinc hydroxide solution, and adds terephthalic acid and polyimide, and obtains filler and filler by ultrasonic reaction and vacuum drying. The amount of addition is controlled at 3-6% of the mass of the polyimide to increase the free volume and mass transfer channel of the gas separation membrane, and the nanocomposite filler is modified by 1-ethyl-3-methylimidazole triflate. , enhance the interaction between inorganic polymer matrix and the affinity of carbon dioxide.
The permeability coefficient and gas separation performance of carbon dioxide are improved, and the rapid transmission and selectivity of carbon dioxide in the film is ensured. The appropriate amount of filler is added to ensure uniform dispersion and mass transfer channels in the film, which may lead to reduced performance when exceeding this amount.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of membrane separation, and in particular to a large-area gas separation membrane and a preparation method thereof. Background Art
[0002] Gas separation membrane technology has been widely used in air separation and purification, recovery of carbon dioxide from combustion exhaust gas and natural gas purification due to its outstanding advantages such as low energy consumption, easy operation and no pollution to the environment. Gas separation membrane materials are the core of gas separation membrane technology, and their performance will directly affect the preparation, separation performance and long-term use performance of gas separation membranes.
[0003] Currently, the commonly used gas separation membranes are divided into three categories: organic membranes, inorganic membranes and mixed matrix membranes. The mixed matrix membrane is a blend of dispersed fillers and continuous polymer matrices. Compared with traditional organic membranes and inorganic membranes, the mixed matrix membrane combines the advantages of organic membranes and inorganic membrane materials. Common metal organic framework filler materials cannot meet the two conditions of large size and ultra-thinness at the same time, and thus it is difficult to construct an effective transfer path for carbon dioxide inside the gas separation membrane material, resulting in poor carbon capture effect. Summary of the invention
[0004] In order to improve the efficiency of carbon dioxide separation, the present invention provides a large-area gas separation membrane and a preparation method thereof.
[0005] The first object of the present invention is to provide a method for preparing a large-area gas separation membrane using the following technical solution: A method for preparing a large-area gas separation membrane comprises the following preparation steps: S1, dissolving zinc nitrate in a solvent, then adding a sodium hydroxide alcohol solution, and reacting under ultrasonic conditions to obtain a zinc hydroxide solution, wherein the molar ratio of the zinc nitrate to the sodium hydroxide is 1:2; S2, then adding a solvent containing terephthalic acid to carry out ultrasonic reaction for 1-2 hours, then filtering the reaction solution to obtain a white precipitate, washing it with ethanol for multiple times, and then vacuum drying it to obtain a filler; S3. Add the filler obtained in step S2 to the solvent and disperse it evenly, then add polyimide and stir evenly to obtain a dispersion, pour the dispersion onto a watch glass, heat at 50-60° C. to evaporate the solvent to obtain a film, and then vacuum dry the film to obtain a gas separation membrane, wherein the amount of the filler added is 3-6% of the mass of the polyimide.
[0006] By adopting the above technical solution, the addition of fillers in the present application increases the free volume in the gas separation membrane and provides additional gas diffusion paths, thereby improving the carbon dioxide permeability coefficient. When the addition amount of the filler is 3-6% of the mass of the polyimide, it can not only ensure the uniform dispersion of the filler in the membrane, but also ensure the mass transfer channel of carbon dioxide in the membrane, thereby improving the separation performance of the gas separation membrane for carbon dioxide and nitrogen. When the addition amount of the filler exceeds 6% of the mass of the polyimide, the filler is likely to agglomerate in the membrane and enhance the crystallinity of the membrane, thereby reducing some mass transfer channels in the gas separation membrane that were originally available for gas molecules to pass through, thereby reducing the gas separation performance of the gas separation membrane.
[0007] Preferably, the mass ratio of terephthalic acid to sodium hydroxide is (60-70):1.
[0008] Preferably, in step S2, the filler is added into ethanol dissolved with 1-ethyl-3-methylimidazolium trifluoromethanesulfonate, and the mixture is stirred and reacted at 55-65° C. for 20-24 hours. The product is then centrifuged and washed, and vacuum dried to obtain a nanocomposite filler.
[0009] Preferably, the mass ratio of the 1-ethyl-3-methylimidazolium trifluoromethanesulfonate to the filler is 1:(1-2).
[0010] Preferably, the concentration of the 1-ethyl-3-methylimidazolium trifluoromethanesulfonate in ethanol is 0.02-0.04 g / ml.
[0011] By adopting the above technical scheme, when the filler is modified by 1-ethyl-3-methylimidazolium trifluoromethanesulfonate to obtain a nanocomposite filler, the interaction between the inorganic filler and the organic polymer matrix is increased, thereby improving the affinity between the two, so that the nanocomposite filler increases the average distance between polymer chain segments, which is conducive to the passage of carbon dioxide gas, and the trifluoromethyl, sulfonic acid group and imidazole group in 1-ethyl-3-methylimidazolium trifluoromethanesulfonate have a strong affinity for carbon dioxide, which increases the carbon dioxide gas transfer sites in the gas separation membrane, and the affinity of the trifluoromethyl, sulfonic acid group and imidazole group for carbon dioxide can promote the dissolution of carbon dioxide in the gas separation membrane, thereby strengthening the dissolution-diffusion mechanism of the gas separation membrane, achieving an improvement in the carbon dioxide permeability coefficient while maintaining a high selectivity.
[0012] Preferably, the solvents in step S1 and step S2 are both N,N-dimethylformamide.
[0013] Preferably, the film is vacuum dried in step S3 at 140-150° C. for 30-32 hours.
[0014] Preferably, the polyimide in step S3 is obtained by the following method: S1. Add 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane to N,N-dimethylformamide and stir to dissolve to form a solution with a concentration of 0.3-0.5 g / ml, then add 0.4-0.5 parts by weight of pyridine and 0.5-0.7 parts by weight of trimethylsilyl chloride and react for 15-20 minutes; S2, adding 1.2-1.5 parts by weight of hexafluorodianhydride and 2-4 parts by weight of N,N-dimethylformamide in an ice water bath and reacting for 15-20 hours; S3. Add 2-2.5 parts by weight of acetic anhydride and 1.5-2.2 parts by weight of pyridine to the solution obtained in step S2, stir and react at room temperature for 6-8 hours, then wash and filter with methanol, and then vacuum dry to obtain polyimide.
[0015] The second objective of the present invention is to provide a gas separation membrane obtained by the above-mentioned method for preparing the large-area gas separation membrane.
[0016] In summary, the present invention has the following beneficial effects: The addition of fillers in the present application increases the free volume in the gas separation membrane and provides additional gas diffusion paths, thereby improving the carbon dioxide permeability coefficient. In particular, when the filler is modified by 1-ethyl-3-methylimidazolium trifluoromethanesulfonate to obtain a nanocomposite filler, the interaction between the inorganic filler and the organic polymer matrix is increased, thereby improving the affinity between the two, so that the nanocomposite filler increases the average distance between polymer chain segments, which is conducive to the passage of carbon dioxide gas. In addition, the trifluoromethyl, sulfonic acid group and imidazole group in 1-ethyl-3-methylimidazolium trifluoromethanesulfonate have a strong interaction with carbon dioxide, which increases the carbon dioxide gas transfer sites in the gas separation membrane. Therefore, the nanocomposite filler strengthens the rapid transfer of carbon dioxide gas in the gas separation membrane.
[0017] The polyimide material obtained by the preparation method of the present application is used in combination with the composite nanomaterial to greatly improve the carbon dioxide gas permeability performance. DETAILED DESCRIPTION
[0018] The present invention is further described in detail below with reference to the embodiments.
[0019] The raw materials used in the preparation examples, embodiments and comparative examples of this application are all commercially available.
[0020] Preparation Example 1 A polyimide comprises the following preparation steps: S1, adding 9g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane to 30ml of N,N-dimethylformamide and stirring to dissolve to form a solution with a concentration of 0.3g / ml, then adding 4g of pyridine and 5g of trimethylsilyl chloride and reacting for 15 minutes; S2, add 12g hexafluorodianhydride and 20g N,N-dimethylformamide in an ice water bath and react for 15h; S3. Add 20 g of acetic anhydride and 15 g of pyridine to the solution obtained in step S2, stir and react at room temperature for 6 hours, then wash and filter with methanol, and then vacuum dry to obtain polyimide.
[0021] Preparation Example 2 A polyimide comprises the following preparation steps: S1. Add 16 g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane to 40 ml of N,N-dimethylformamide and stir to dissolve to form a solution with a concentration of 0.4 g / ml. Then add 4.5 g of pyridine and 6 g of trimethylsilyl chloride and react for 20 minutes. S2, add 13g hexafluorodianhydride and 30g N,N-dimethylformamide in an ice water bath and react for 18h; S3. Add 22 g of acetic anhydride and 18 g of pyridine to the solution obtained in step S2, stir and react at room temperature for 7 hours, then wash and filter with methanol, and then vacuum dry to obtain polyimide.
[0022] Preparation Example 3 A polyimide comprises the following preparation steps: S1. Add 25 g of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane to 50 ml of N,N-dimethylformamide and stir to dissolve to form a solution with a concentration of 0.5 g / ml, then add 5 g of pyridine and 7 g of trimethylsilyl chloride, and react for 20 minutes; S2, add 15g hexafluorodianhydride and 4g N,N-dimethylformamide in an ice water bath and react for 20h; S3. Add 25 g of acetic anhydride and 22 g of pyridine to the solution obtained in step S2, stir and react at room temperature for 8 hours, then wash and filter with methanol, and then vacuum dry to obtain polyimide.
[0023] Example 1 A method for preparing a large-area gas separation membrane comprises the following preparation steps: S1. Dissolve 3.86 g of zinc nitrate hexahydrate in 6 ml of N,N-dimethylformamide solution, then add sodium hydroxide alcohol solution (dissolve 1.04 g of sodium hydroxide in 3 ml of methanol), and react under ultrasonic conditions to obtain a zinc hydroxide solution, wherein the molar ratio of zinc nitrate to sodium hydroxide is 1:2; S2, then add N, N-dimethylformamide solution containing terephthalic acid (dissolve 62.4 g terephthalic acid in 1.9 L N, N-dimethylformamide) and carry out ultrasonic reaction for 1 hour, then filter and separate the reaction solution to obtain a white precipitate, wash it with ethanol several times, and then vacuum dry it to obtain a filler, the mass ratio of terephthalic acid to sodium hydroxide is 60:1; S3. Take 0.15 g of the filler obtained in step S2 and add it to 50 ml of N,N-dimethylformamide to disperse evenly. Then add 5 g of the polyimide obtained in Preparation Example 1 and stir evenly to obtain a dispersion. Pour the dispersion onto a watch glass and heat it at 50°C to evaporate the solvent to obtain a film. Then vacuum dry the film at 140°C for 30 hours to obtain a gas separation membrane, wherein the amount of filler added is 3% of the mass of the polyimide.
[0024] Example 2 A method for preparing a large-area gas separation membrane comprises the following preparation steps: S1. Dissolve 3.86 g of zinc nitrate hexahydrate in 6 ml of N,N-dimethylformamide solution, then add sodium hydroxide alcohol solution (dissolve 1.04 g of sodium hydroxide in 3 ml of methanol), and react under ultrasonic conditions to obtain a zinc hydroxide solution, wherein the molar ratio of zinc nitrate to sodium hydroxide is 1:2; S2, then add N, N-dimethylformamide solution containing terephthalic acid (dissolve 67.6 g terephthalic acid in 1.95 L N, N-dimethylformamide) and carry out ultrasonic reaction for 1 hour, then filter and separate the reaction solution to obtain a white precipitate, wash it with ethanol several times, and then vacuum dry it to obtain a filler, the mass ratio of terephthalic acid to sodium hydroxide is 65:1; S3. Take 0.2 g of the filler obtained in step S2 and add it to 50 ml of N,N-dimethylformamide to disperse evenly. Then add 5 g of the polyimide obtained in Preparation Example 1 and stir evenly to obtain a dispersion. Pour the dispersion onto a watch glass and heat it at 55°C to evaporate the solvent to obtain a film. Then vacuum dry the film at 150°C for 32 hours to obtain a gas separation membrane, wherein the amount of filler added is 4% of the mass of the polyimide.
[0025] Example 3 A method for preparing a large-area gas separation membrane comprises the following preparation steps: S1. Dissolve 3.86 g of zinc nitrate hexahydrate in 6 ml of N,N-dimethylformamide solution, then add sodium hydroxide alcohol solution (dissolve 1.04 g of sodium hydroxide in 3 ml of methanol), and react under ultrasonic conditions to obtain a zinc hydroxide solution, wherein the molar ratio of zinc nitrate to sodium hydroxide is 1:2; S2, then add N, N-dimethylformamide solution containing terephthalic acid (dissolve 72.8 g terephthalic acid in 2 L N, N-dimethylformamide) and carry out ultrasonic reaction for 1 hour, then filter and separate the reaction solution to obtain a white precipitate, wash it with ethanol several times, and then vacuum dry it to obtain a filler, the mass ratio of terephthalic acid to sodium hydroxide is 70:1; S3. Take 0.3 g of the filler obtained in step S2 and add it to 50 ml of N,N-dimethylformamide to disperse evenly. Then add 5 g of the polyimide obtained in Preparation Example 1 and stir evenly to obtain a dispersion. Pour the dispersion onto a watch glass and heat it at 60°C to evaporate the solvent to obtain a film. Then vacuum dry the film at 150°C for 30 hours to obtain a gas separation membrane, wherein the amount of filler added is 6% of the mass of the polyimide.
[0026] Example 6 A method for preparing a large-area gas separation membrane comprises the following preparation steps: S1. Dissolve 3.86 g of zinc nitrate hexahydrate in 6 ml of N,N-dimethylformamide solution, then add sodium hydroxide alcohol solution (dissolve 1.04 g of sodium hydroxide in 3 ml of methanol), and react under ultrasonic conditions to obtain a zinc hydroxide solution, wherein the molar ratio of zinc nitrate to sodium hydroxide is 1:2; S2, then add N, N-dimethylformamide solution containing terephthalic acid (dissolve 67.6 g terephthalic acid in 1.95 L N, N-dimethylformamide) and carry out ultrasonic reaction for 1 hour, then filter and separate the reaction solution to obtain a white precipitate, wash it with ethanol several times, and then vacuum dry it to obtain a filler, the mass ratio of terephthalic acid to sodium hydroxide is 65:1; S3, taking 5 g of the filler obtained in step S2, adding it to ethanol dissolved with 1-ethyl-3-methylimidazolium trifluoromethanesulfonate (5 g of 1-ethyl-3-methylimidazolium trifluoromethanesulfonate was dissolved in 250 ml of ethanol, that is, the mass ratio of 1-ethyl-3-methylimidazolium trifluoromethanesulfonate to the filler was 1:1), stirring and reacting at 55° C. for 20 hours, then centrifuging and washing the product, and vacuum drying to obtain a nanocomposite filler; S4. Take 0.2 g of the nanocomposite filler obtained in step S3 and add it to 50 ml of N,N-dimethylformamide to disperse it evenly. Then add 5 g of the polyimide obtained in Preparation Example 1 and stir evenly to obtain a dispersion. Pour the dispersion onto a watch glass and heat it at 55° C. to evaporate the solvent to obtain a film. Then, vacuum dry the film at 150° C. for 32 hours to obtain a gas separation membrane, wherein the amount of the nanocomposite filler added is 4% of the mass of the polyimide.
[0027] Example 7 A method for preparing a large-area gas separation membrane comprises the following preparation steps: S1. Dissolve 3.86 g of zinc nitrate hexahydrate in 6 ml of N,N-dimethylformamide solution, then add sodium hydroxide alcohol solution (dissolve 1.04 g of sodium hydroxide in 3 ml of methanol), and react under ultrasonic conditions to obtain a zinc hydroxide solution, wherein the molar ratio of zinc nitrate to sodium hydroxide is 1:2; S2, then add N, N-dimethylformamide solution containing terephthalic acid (dissolve 67.6 g terephthalic acid in 1.95 L N, N-dimethylformamide) and carry out ultrasonic reaction for 1 hour, then filter and separate the reaction solution to obtain a white precipitate, wash it with ethanol several times, and then vacuum dry it to obtain a filler, the mass ratio of terephthalic acid to sodium hydroxide is 65:1; S3, taking 10g of the filler obtained in step S2, adding it to ethanol dissolved with 1-ethyl-3-methylimidazolium trifluoromethanesulfonate (5g of 1-ethyl-3-methylimidazolium trifluoromethanesulfonate was dissolved in 125ml of ethanol, that is, the mass ratio of 1-ethyl-3-methylimidazolium trifluoromethanesulfonate to the filler was 1:2), stirring and reacting at 65°C for 24 hours, then centrifuging and washing the product, and vacuum drying to obtain a nanocomposite filler; S4. Take 0.2 g of the nanocomposite filler obtained in step S3 and add it to 50 ml of N,N-dimethylformamide to disperse it evenly. Then add 5 g of the polyimide obtained in Preparation Example 1 and stir evenly to obtain a dispersion. Pour the dispersion onto a watch glass and heat it at 55° C. to evaporate the solvent to obtain a film. Then, vacuum dry the film at 150° C. for 32 hours to obtain a gas separation membrane, wherein the amount of the nanocomposite filler added is 4% of the mass of the polyimide.
[0028] Comparative Example 1 A method for preparing a large-area gas separation membrane is different from Example 2 in that the amount of filler added is 2% of the mass of polyimide, that is, the amount of filler added is 0.1g, and the amount of polyimide added is 5g, and the rest are the same as Example 2.
[0029] Comparative Example 2 A method for preparing a large-area gas separation membrane is different from Example 2 in that the amount of filler added is 7% of the mass of polyimide, that is, the amount of filler added is 0.35g, and the amount of polyimide added is 5g, and the rest are the same as Example 2.
[0030] Performance Test The gas separation membranes obtained in the above embodiments and comparative examples were used to detect the permeation of carbon dioxide and nitrogen, wherein the volume ratio of carbon dioxide to nitrogen was 1:1, and the detection was based on the standard GB / T40260-2021 "Test Method for Gas Permeability of Polymer Membrane Materials". The test results are shown in Table 1.
[0031] Table 1 Gas separation membrane permeability test results project <![CDATA[P 二氧化碳 ]]> <![CDATA[P 氮气 ]]> <![CDATA[α 二氧化碳 / 氮气 ]]> Example 1 27.32 1.79 15.25 Example 2 28.86 1.78 16.21 Example 3 28.41 1.80 15.78 Example 4 29.65 1.78 16.65 Example 5 28.94 1.75 16.54 Example 6 30.45 1.73 17.58 Example 7 30.36 1.74 17.41 Comparative Example 1 21.41 2.03 10.54 Comparative Example 2 20.56 2.11 9.76 The unit of the permeability coefficients of carbon dioxide and nitrogen in the above table is Barrer.
[0032] It can be seen from Table 1 that when the gas separation membranes obtained in Examples 1-3 of the present application are used to separate and detect a mixed gas of carbon dioxide and nitrogen, the permeability coefficient of carbon dioxide shows a trend of first increasing and then decreasing. This indicates that when the addition amount of each substance in the present application is within the range specified in the present application, the selectivity of the gas separation membrane for carbon dioxide can be effectively improved.
[0033] Compared with Example 2, when the polyimide used was the polyimide obtained in Preparation Example 2 and Preparation Example 3, the carbon dioxide permeability coefficients in Examples 4 and 5 were better than that in Example 2, and the separation coefficient α of carbon dioxide and nitrogen was 二氧化碳 / 氮气 It is also higher than the separation coefficient α of carbon dioxide and nitrogen in Example 2 二氧化碳 / 氮气 It can be seen that the addition amount of each substance in Preparation Example 2 and Preparation Example 3 can further improve the selectivity of the gas separation membrane to carbon dioxide.
[0034] Compared with Example 2, when the filler in step S2 is modified with 1-ethyl-3-methylimidazole trifluoromethanesulfonate, the gas separation membrane obtained in Example 6-7 has further improved preferential selection performance for carbon dioxide, and the permeability coefficient of carbon dioxide is further improved. The reason may be that after the inorganic filler is modified with 1-ethyl-3-methylimidazole trifluoromethanesulfonate, the dispersion performance of the inorganic filler in the organic polymer membrane is improved, and the interface compatibility problem between the organic-inorganic filler is improved. In addition, after the filler is modified with 1-ethyl-3-methylimidazole trifluoromethanesulfonate, it can interfere with the arrangement and stacking of the polymer chain segments, and at the same time provide additional carbon dioxide mass transfer channels, increase the polymer molecular chain spacing and carbon dioxide transfer sites in the gas separation membrane, and strengthen the diffusion process of carbon dioxide in the gas separation membrane.
[0035] Compared with Example 2, when the amount of filler added is not within the range specified in the present application, the selectivity of the gas separation membranes obtained in Examples 1 and 2 for carbon dioxide is reduced, resulting in a decrease in the permeability coefficient of carbon dioxide. It can be seen that when the amount of filler added is lower or higher than the range specified in the present application, the permeability of carbon dioxide will be reduced. The reason may be that when the content of filler is too high, agglomeration will occur in the membrane and the crystallinity of the membrane will be enhanced, thereby reducing some mass transfer channels in the gas separation membrane that were originally available for gas molecules to pass through, thereby reducing the gas separation performance of the gas separation membrane.
[0036] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a large-area gas separation membrane, It is characterized in that The method comprises the following preparation steps: S1, dissolving zinc nitrate in a solvent, then adding a sodium hydroxide alcohol solution, and reacting under ultrasonic conditions to obtain a zinc hydroxide solution, wherein the molar ratio of the zinc nitrate to the sodium hydroxide is 1:2; S2, then adding a solvent containing terephthalic acid to carry out ultrasonic reaction for 1-2 hours, then filtering the reaction solution to obtain a white precipitate, washing it with ethanol for multiple times, and then vacuum drying it to obtain a filler; S3. Add the filler obtained in step S2 to the solvent and disperse it evenly, then add polyimide and stir evenly to obtain a dispersion, pour the dispersion onto a watch glass, heat at 50-60° C. to evaporate the solvent to obtain a film, and then vacuum dry the film to obtain a gas separation membrane, wherein the amount of the filler added is 3-6% of the mass of the polyimide.
2. The method for preparing a large-area gas separation membrane according to claim 1, Features: The mass ratio of terephthalic acid to sodium hydroxide is (60-70):
1.
3. The method for preparing a large-area gas separation membrane according to claim 1, Features: In the step S2, the filler is added into ethanol dissolved with 1-ethyl-3-methylimidazolium trifluoromethanesulfonate, and the mixture is stirred and reacted at 55-65° C. for 20-24 hours. The product is then centrifuged, washed, and vacuum dried to obtain a nanocomposite filler.
4. The method for preparing a large-area gas separation membrane according to claim 3, Features: The mass ratio of the 1-ethyl-3-methylimidazolium trifluoromethanesulfonate to the filler is 1:(1-2).
5. The method for preparing a large-area gas separation membrane according to claim 3, Features: The concentration of the 1-ethyl-3-methylimidazolium trifluoromethanesulfonate in ethanol is 0.02-0.04 g / ml.
6. The method for preparing a large-area gas separation membrane according to claim 1, Features: The solvents in step S1 and step S2 are both N,N-dimethylformamide.
7. The method for preparing a large-area gas separation membrane according to claim 1, Features: The film is vacuum dried in step S3 at 140-150° C. for 30-32 hours.
8. The method for preparing a large-area gas separation membrane according to claim 1, Features: In step S3, the polyimide is obtained by the following method: S1. Add 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane to N,N-dimethylformamide and stir to dissolve to form a solution with a concentration of 0.3-0.5 g / ml, then add 0.4-0.5 parts by weight of pyridine and 0.5-0.7 parts by weight of trimethylsilyl chloride and react for 15-20 minutes; S2, adding 1.2-1.5 parts by weight of hexafluorodianhydride and 2-4 parts by weight of N,N-dimethylformamide in an ice water bath and reacting for 15-20 hours; S3. Add 2-2.5 parts by weight of acetic anhydride and 1.5-2.2 parts by weight of pyridine to the solution obtained in step S2, stir and react at room temperature for 6-8 hours, then wash and filter with methanol, and then vacuum dry to obtain polyimide.
9. A gas separation membrane obtained by the method for preparing a large-area gas separation membrane according to any one of claims 1 to 8.
Citation Information
Patent Citations
Preparation method of gas separation membrane with high MOF filler content
CN110639374A
Preparation method of fluorine-containing polyimide film for gas separation
CN114854060A
Ionic liquid modified ZnBDC / polymer mixed matrix membrane for gas separation and preparation method of ionic liquid modified ZnBDC / polymer mixed matrix membrane
CN117018875A
Preparation method and application of polyester supported ionic liquid doped polyimide mixed matrix membrane
CN118286894A
Treated mixed matrix polymeric membranes