Preparation method of 3D printing monolithic catalyst, 3D printing monolithic catalyst and application of 3D printing monolithic catalyst

The preparation of magnesium-based lanthanum hexaluminate monolithic catalyst through 3D printing technology solved the problems of large flow resistance of particulate catalysts and unsuitable sintering temperature of the integral catalysts, achieved efficient decomposition of liquid propellant N2O, simplified the installation process, and improved the catalyst Structural strength and specific surface area.

CN118874455APending Publication Date: 2024-11-01NAT UNIV OF DEFENSE TECH

Patent Information

Application Number
CN202410975518.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the single-component engine, existing granular catalysts have problems such as large flow resistance, cumbersome installation, severe wear and easy to break the coating. In the integrated catalyst, the carrier strength is poor or the specific surface area is insufficient when the sintering temperature is not appropriate, which affects the catalytic performance.

Method used

Magnesium-based lanthanum hexaluminate was prepared as a catalyst support by synthesis of magnesium-based lanthanum hexaluminate raw material powder mixed with photocuring resin, designing a masonry-shaped three-dimensional structure, and controlling the sintering process to carbonize in an inert atmosphere and in air Carbon is removed under the atmosphere to form a porous structure, and the specific surface area and support strength are improved.

Benefits of technology

An integrated catalyst with high structural strength and specific surface area under high temperature and high pressure conditions is realized, which improves the decomposition efficiency of liquid propellant N2O, simplifies the installation steps and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874455A_ABST
    Figure CN118874455A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a 3D printing monolithic catalyst, the 3D printing monolithic catalyst and application of the 3D printing monolithic catalyst, and the method comprises the following steps: uniformly mixing raw material powder for synthesizing magnesium-based lanthanum hexaaluminate with light-cured resin to obtain 3D printing slurry; printing the 3D printing slurry into a monolithic catalyst green body with a corresponding shape through a 3D printer, and calcining the monolithic catalyst green body according to a sintering process to obtain a monolithic catalyst carrier; the sintering process comprises the following steps: sintering and carbonizing in an inert atmosphere, and then removing carbon in an air atmosphere; and loading an active substance on the monolithic catalyst carrier to obtain the monolithic catalyst. The method can be used for generating 3D printing magnesium-based lanthanum hexaaluminate with certain structural strength and relatively high specific surface area as a catalyst carrier, and the 3D printing magnesium-based lanthanum hexaaluminate is applied to a spaceflight monopropellant engine, so that efficient decomposition of a liquid propellant N2O is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the cross-technical field of 3D printing and catalysts, and in particular to a method for preparing a 3D printed monolithic catalyst, a 3D printed monolithic catalyst and applications thereof. Background Art

[0002] Space monopropellant engines are widely used in my country's space stations, manned spacecraft, spacecraft orbits, attitude control and other fields. Among them, the catalyst decomposes the liquid propellant to burn and produce the propellant gas, which is the entire power source of the engine. Therefore, the catalytic decomposition performance of the catalyst for liquid propellant is a key factor in determining the engine's propulsion performance and stability.

[0003] At present, the mainstream catalysts used in monopropellant engines are often mainly granular catalysts. The interior of the granular bed is composed of small granular catalysts tightly stacked. The gaps between the particles constitute the flow channel of the propellant. The channels inside the granular bed are complex and tortuous, and the laminar flow resistance is large, making it difficult for the propellant to flow. At the same time, the installation steps and use requirements of granular catalysts are very cumbersome and strict. While ensuring the filling regularity, it is also necessary to ensure that the gas-liquid flow resistance inside the engine meets the use requirements. Affected by extreme use conditions, the particles often suffer from severe wear and even breakage, which leads to the formation of holes inside the catalytic bed and overflow of the propeller; broken particles will block the nozzle after entering the throat of the engine, causing the chamber pressure to exceed the rated value, seriously affecting the safety of the aircraft. In order to fix the small-volume catalyst particles, a mesh baffle is often used at the end of the combustion chamber for fixation. Under high temperature and high pressure conditions, the corrosion of the baffle has also become an important factor hindering the development of granular catalysts.

[0004] As a one-piece catalyst, the monolithic catalyst can be autonomously regulated in its internal pore structure compared to the traditional granular bed. The interconnected pores shorten the diffusion distance of the propellant, making the internal flow of the monolithic bed more uniform, and greatly improving the mass transfer and heat transfer performance. The integrated design, while getting rid of the baffle restriction, greatly simplifies the catalyst installation steps and saves a lot of manpower and material resources. At present, the commonly used monolithic catalysts are mainly honeycomb beds and foam beds. The honeycomb bed is mainly made of ceramic materials as carriers, and is prepared by extrusion molding and coating. It has the advantages of simple preparation process and high carrier strength. However, due to the limitation of the extrusion molding preparation process, the honeycomb bed only has radially interconnected pores and unidirectional liquid flow, and mass transfer cannot occur in the lateral direction. The heat transfer process can only be achieved by conduction through the channel wall, which is prone to stress concentration and carrier damage. At the same time, the specific surface area of ​​the ceramic material constituting the carrier is generally low, and it is impossible to load the required amount of active ingredients. Therefore, coating is often used to increase the load. However, the coating with low binding force is prone to breakage and falling off under extreme conditions. These deficiencies hinder the further development of the honeycomb bed. The foam bed is an integral catalyst prepared by foaming. Common skeleton materials include metal, ceramic, carbon, etc. The porosity of the foam bed is more uniform, and the network structure formed enables it to have three-dimensional mass transfer capabilities, overcoming the shortcomings of the honeycomb bed. At the same time, the adjustability of the porosity has significantly improved its specific surface area and space utilization. However, due to the uncontrollability of the foaming process, the catalyst produced by each foaming is random and not reproducible. The skeleton produced by foaming is also affected by the foaming process. The length and diameter of the generated rods are unevenly distributed, and there is still a risk of breakage in weak areas.

[0005] In recent years, with the continuous breakthroughs in 3D printing technology and the further expansion of its application fields, various products prepared by 3D printing have been further developed in the fields of energy, chemical industry, environment, aerospace, etc. In the field of catalysis, 3D printing technology has completely changed the limitations of the structural design of monolithic catalysts through its unique independent structural design and subtractive manufacturing methods. The monolithic catalyst used in monocomponent engines can be designed and printed according to the requirements of mass transfer, heat transfer, gas-liquid flow resistance inside different types of engines, combined with computer topological structure optimization and fluid simulation calculations, to design and print monolithic catalysts with complex structures and superior performance, thereby reducing production costs and shortening production cycles.

[0006] But at the same time, the monolithic catalyst prepared by 3D printing also faces a practical application difficulty, that is, during the sintering and ceramicization process of the powder raw material, if the sintering temperature is low, the carrier strength is poor; if the sintering temperature is too high, the specific surface area of ​​the catalyst carrier will drop sharply, the active metal loading will decrease, and the catalytic performance will decrease. Therefore, how to prepare a monolithic catalyst with a certain structural strength, a high specific surface area, and the materials used meet the requirements of the use scenario has become an urgent problem to be solved. Summary of the invention

[0007] The present invention provides a preparation method of a 3D printed monolithic catalyst, a 3D printed monolithic catalyst and an application thereof, which are used to generate a 3D printed magnesium-based lanthanum hexaaluminate with certain structural strength and high specific surface area as a catalyst carrier, which is used in aerospace monocomponent engines to achieve efficient decomposition of liquid propellant N2O, and provide new ideas for the catalytic ignition method of the monocomponent engine.

[0008] To achieve the above object, the present invention provides a method for preparing a 3D printed monolithic catalyst, comprising the following steps:

[0009] S1. Evenly mix the raw material powder of synthesized magnesium-based lanthanum hexaaluminate with the photocurable resin to obtain a 3D printing slurry.

[0010] The photocurable resin includes: a photocurable monomer, an inhibitor, a photoinitiator and a lubricant.

[0011] Among them, the basic unit structure of the three-dimensional model is a masonry structure, a body-centered cubic structure and a face-centered cubic structure, which are flexible, high-strength and widely applicable. The corresponding three-dimensional structure is designed in combination with the internal structure and size of the monopropellant engine. Figure 1 As shown, it is a schematic diagram of a three-dimensional model of a type of structure of the present invention. Figure 1 It is a body-centered cubic structure.

[0012] S2, designing a three-dimensional model with a pore structure, importing the three-dimensional model into a 3D printer and performing slicing processing;

[0013] S3. Print the 3D printing slurry into a monolithic catalyst green body of corresponding shape through a 3D printer, and test the TG-DSC curve of the monolithic catalyst green body. Combined with the synthesis process of magnesium-based lanthanum hexaaluminate, determine the sintering process of the monolithic catalyst green body, and then calcine the monolithic catalyst green body according to the sintering process to obtain a monolithic catalyst carrier.

[0014] Among them, the sintering process is: first sintering and carbonization in an inert atmosphere, and then decarbonization in an air atmosphere. The purpose of this is: first sintering in an inert atmosphere to carbonize the light-curing resin to wrap the raw material powder, and then the wrapped raw material powder is synthesized into magnesium-based lanthanum hexaaluminate. The magnesium-based lanthanum hexaaluminate product synthesized in this way has a low density and a small particle size, which can increase the specific surface area and the active material loading content to a certain extent. A section of oxidation sintering is added later to remove the carbon coated on the surface of the powder. Decarbonization will form a porous structure in the carrier, increase the contact sites of nitrous oxide, and improve the conversion rate.

[0015] S4, loading the monolithic catalyst carrier with active substances to obtain a monolithic catalyst.

[0016] The present invention proposes a method for preparing a 3D printed monolithic catalyst, wherein a 3D printed slurry prepared from a magnesium-based lanthanum hexaaluminate raw material powder is printed at one time into a three-dimensional monolithic structure, and then a catalyst carrier is generated by a solid phase reaction while sintering and debinding by controlling the sintering process, and finally an active metal is loaded by impregnation to obtain a monolithic catalyst. The method has a simple preparation process and can achieve batch production; the 3D printed structure can be optimized and improved by combining computer topological structure optimization and fluid simulation calculation, and the weight of the carrier can be reduced while improving its structural strength and contact area. At the same time, the structure can be customized according to the required structure. The monolithic catalyst obtained by 3D printing has high structural precision and high strength, and can be quickly and stably prepared as a monolithic catalyst, saving materials and increasing production speed. The monolithic structure is formed at one time without assembly and secondary processing; the loaded active components can be adjusted according to the type and concentration of the liquid propellant actually used, and the flexibility is high; the monolithic catalyst is easy to install, saving a lot of manpower and material resources.

[0017] Preferably, in step S1, the photocurable monomer is one or more of 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, and dicyclopentenyl methacrylate, accounting for 60-90wt% of the mass fraction of the photocurable resin;

[0018] Preferably, in step S1, the polymerization inhibitor is one or more of p-hydroxyphenyl ether, hydroquinone, tert-butylcatechol and copper cyclohexane, accounting for 0.5-1wt% of the mass fraction of the photocurable resin;

[0019] Preferably, in step S1, the photoinitiator is one or more of Irgacure 184, TPO, DMPA, and photoinitiator 819, accounting for 3-5wt% of the mass fraction of the photocurable resin;

[0020] Preferably, in step S1, the lubricant is one or more of polyethylene glycol, oleic acid, stearic acid, and trioctylphosphine oxide, accounting for 1-5wt% of the mass fraction of the photocurable resin;

[0021] Preferably, in step S1, after the photocurable resin and raw material powder are mixed into 3D printing slurry, the raw material powder accounts for 50-55wt% of the 3D printing slurry.

[0022] Preferably, the preparation process of the raw material powder for synthesizing magnesium-based lanthanum hexaaluminate in step S1 is as follows:

[0023] Weigh a certain mass ratio of nano-alumina powder, nano-magnesium oxide powder and nano-lanthanum oxide powder, add a certain proportion of defoaming agent and adhesive, add an appropriate amount of dispersant to dissolve, mechanically stir evenly to obtain a solution suitable for spray drying granulation, then perform centrifugal spray drying granulation, sieve, and prepare a raw material mixed powder with a suitable particle size.

[0024] Among them, the particle sizes of nano-alumina powder, nano-magnesium oxide powder and nano-lanthanum oxide powder are all 40-50nm; the particle size of nano-oxide powder is 40-50nm, which is convenient for subsequent granulation treatment.

[0025] The particle size U90% of the raw material mixed powder after spray drying, granulation and sieving is 1-10 μm, and the maximum particle size does not exceed 75 μm.

[0026] Preferably, in step S1, the mass ratio of nano-alumina powder, nano-magnesium oxide powder and nano-lanthanum oxide powder is (13-14):1:(4-4.5).

[0027] Preferably, in step S1, the mass proportion of the defoaming agent is 0.5-1.0% of the total mass of the nano-alumina powder, the nano-magnesium oxide powder and the nano-lanthanum oxide powder;

[0028] The mass proportion of the binder is 1-3% of the total mass of the nano-alumina powder, the nano-magnesia powder and the nano-lanthanum oxide powder.

[0029] The above mass ratio is set to ensure the granulation effect without affecting the performance of the subsequent printing slurry.

[0030] In the solution suitable for spray drying granulation, the total mass ratio of nano-alumina powder, nano-magnesium oxide powder and nano-lanthanum oxide powder to the mass ratio of dispersant is 1: (3-5). If the dispersant content is too high, the granulation time will be too long, and if the dispersant content is too low, the solution will be viscous and easy to clog the granulation equipment.

[0031] Preferably, in step S1, the defoaming agent is one or more of triammonium citrate, polydimethylsilane, and tributyl phosphate;

[0032] The binder is one or more of gum arabic, ethyl cellulose and povidone;

[0033] The dispersant is one or more of water and anhydrous ethanol.

[0034] Preferably, in step S3, the sintering process is as follows:

[0035] Carbonization sintering in inert atmosphere:

[0036] 1) From room temperature to 220-240℃, the heating rate is 0.4-0.6℃ / min, and the insulation time is 1-2h;

[0037] 2) From 220-240℃ to 280-300℃, the heating rate is 0.4-0.6℃ / min, and the insulation time is 1-2h;

[0038] 3) From 280-300℃ to 420-440℃, the heating rate is 0.4-0.6℃ / min, and the insulation time is 1-2h;

[0039] 4) From 420-440℃ to 480-500℃, the heating rate is 0.4-0.6℃ / min, and the insulation time is 1-2h;

[0040] 5) From 480-500℃ to 1300-1400℃, the heating rate is 2-4℃ / min, and the insulation time is 4-8h;

[0041] Carbon removal in air atmosphere:

[0042] 6) From room temperature to 800-1000℃, the heating rate is 5-10℃ / min, and the insulation time is 20-28h.

[0043] It can be seen that the temperature is raised in stages under an inert atmosphere. The advantage of raising the temperature in stages is that each different component in the photocurable resin material can be carbonized at a suitable temperature, such as: stage 1) carbonization of the photoinitiator; stage 2) carbonization of the photocurable monomer; stage 3) carbonization of the lubricant; stage 4) carbonization of the inhibitor. Then, the temperature can be raised in one step under an air atmosphere, and the carbon can be removed after reaching a certain temperature. Specifically, stages 1)-4) are to carbonize the cured resin, 900-950℃ raw material powder generates metastable MgAl2O4 and LaAlO3, and 1300-1450℃ generates stable LaMgAl 11 O 19 . Carbon sintering in air atmosphere generates carbon dioxide and is removed. The detailed reaction equation is as follows:

[0044] 900-950℃:

[0045] La2O3+Al2O3=2LaAlO3;

[0046] MgO+Al2O3=MgAl2O4;

[0047] 1300-1450℃:

[0048] LaAlO3+MgAl2O4+4Al2O4=LaMgAl 11 O 19 .

[0049] The heating process is continuous throughout the sintering process, but the heating speed is different at different stages. The temperature before 500℃ is to carbonize the resin material, and the temperature after 500℃ is to synthesize magnesium-based lanthanum hexaaluminate and sinter the powder into a whole. In the process of heating from 500℃ to 1450℃, solid phase reaction will occur. LaAlO3 will be generated at around 900-950℃, and LaMgAl will continue to react when the temperature is raised to 1300-1450℃. 11 O 19 .

[0050] Preferably, step S4 specifically includes:

[0051] The monolithic catalyst carrier is immersed in a 5-10% by mass liquid chloroiridic acid, and after immersion for 30-40 minutes, it is taken out and dried in an oven at above 80° C. for 30-60 minutes until the surface is completely dry;

[0052] Then roast at 400-450°C in air atmosphere, keep warm for 1-2 hours, and repeat oxidation roasting 5-10 times;

[0053] Then, the product is reduced at 300-350° C. in a hydrogen atmosphere for 1-2 hours to obtain the final finished monolithic catalyst.

[0054] The present invention also provides a 3D printed integral catalyst, which is prepared by the above preparation method.

[0055] The present invention also proposes an application of a 3D printed monolithic catalyst, wherein the 3D printed monolithic catalyst or the 3D printed monolithic catalyst prepared by the above-mentioned preparation method is applied to the decomposition of liquid propellant N2O.

[0056] The 3D printed integral catalyst prepared by the above-mentioned preparation method proposed in the present invention has high catalyst structural strength and catalytic activity and good high temperature resistance, and is suitable for high temperature and high pressure conditions of monocomponent engines.

[0057] The application of the above-mentioned 3D printed monolithic catalyst proposed in the present invention in the catalytic decomposition reaction of N2O can effectively solve the difficulties of existing granular catalysts such as large laminar flow resistance and insufficient mechanical strength. At the same time, the method of directly loading active ingredients avoids the risk of coating shedding. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 It is a schematic diagram of a three-dimensional model of a body-centered cubic structure of the present invention;

[0059] Figure 2 TG-DSC curve of the green body at 1500° C. in Example 1 of the present invention;

[0060] Figure 3 is the sintering curve of the green body in Example 1 of the present invention;

[0061] Figure 4 This is a SEM image of the printed material carrier obtained in Example 1 of the present invention;

[0062] Figure 5 This is a SEM image of the printed material carrier obtained in Comparative Example 1 of the present invention;

[0063] Figure 6 This is a SEM image of the printed part carrier obtained in Comparative Example 2 of the present invention;

[0064] Figure 7 This is a SEM image of the printed part carrier obtained in Comparative Example 3 of the present invention;

[0065] Figure 8 The N2O decomposition rate curves of the finished monolithic catalysts obtained in Example 1 of the present invention and Comparative Examples 1 to 3 are shown. DETAILED DESCRIPTION

[0066] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0067] Embodiment 1:

[0068] Step 1: Use the 3D modeling software Soilworks to create a corresponding 3D model with a pore structure, such as Figure 1 As shown, the body-centered cubic structure. After the three-dimensional model is converted into STL format, it is imported into the 3D printer, and the slice thickness is determined to be 0.13 mm according to the curing depth and curing time of the slurry.

[0069] Step 2: Prepare the photocurable 3D printing slurry. Prepare the powder materials of the synthetic carrier, nano-alumina, nano-magnesium oxide, and nano-lanthanum oxide, in a ratio of 14:1:4, totaling 800g. Then add 6.4g of triammonium citrate as a defoamer at 0.8% of the powder mass, 24g of gum arabic as a binder at 2% of the powder mass, and finally add 2.4kg of water 3 times the mass of the powder as a solvent. Use a mechanical stirring device to mix evenly. Finally, use a spray granulator for granulation. The granulated powder is sieved through a 200-mesh sieve to obtain a powder raw material with a particle size of less than 75μm. Take 500g of the powder raw material, add 450g of 4-hydroxybutyl acrylate, 5g of p-hydroxyphenyl ether, 22.5g of TPO, and 22.5g of polyethylene glycol, mix evenly, and prepare a photocurable 3D printing slurry with a mass fraction of 50wt%.

[0070] Step 3: Use a light-curing 3D printing device to print the green body of the corresponding structure and use alcohol to clean it. Figure 2 As shown, after testing the TG-DSC curve of the green body, according to the TG-DSC curve and the high temperature solid phase synthesis process of magnesium-based lanthanum hexaaluminate, as shown in FIG. Figure 3 As shown, the final sintering temperature of the green body is set to 1350°C, the holding time is 6h, and the detailed heating system is:

[0071] Stage 1) Room temperature—230°C, heating rate 0.5°C / min, holding time 1h, Ar atmosphere;

[0072] Stage 2) 230-290°C, heating rate 0.5°C / min, holding time 1h, Ar atmosphere;

[0073] Stage 3) 290-430°C, heating rate 0.5°C / min, holding time 1h, Ar atmosphere;

[0074] Stage 4) 430-500°C, heating rate 0.5°C / min, holding time 1h, Ar atmosphere;

[0075] Stage 5) 500-1350°C, heating rate 3°C / min, holding time 6h, Ar atmosphere;

[0076] Stage 6) Room temperature - 900 °C, heating rate 8 °C / min, holding time 24 h, air atmosphere;

[0077] The measured shrinkage of the green test sample after calcination was 18.20% in the X and Y axis directions and 21.00% in the Z axis direction. The model was enlarged according to the shrinkage of the X, Y and Z axes, and then the green formal sample was sintered according to the above sintering process to obtain the final printed part carrier. Figure 4 As shown, a SEM image of the printed part carrier obtained in Example 1 is provided.

[0078] Step 4: Soak the sintered carrier in the prepared loaded liquid chloroiridic acid, soak for 30 minutes, take it out, and dry it in an 80℃ oven for 30 minutes. Then place it in a medium-temperature tube furnace, bake it at 400℃ in an air atmosphere, keep it warm for 1 hour, and repeat the oxidation baking 5 times. Put the carrier after 5 bakings into a vacuum multifunctional experimental furnace, reduce it at 300℃ in a hydrogen atmosphere, and keep it warm for 1 hour. The final finished monolithic catalyst is obtained.

[0079] Comparative Example 1:

[0080] Step 1 and step 2 are the same as in Example 1.

[0081] Step 3: Use the light-curing 3D printing equipment to print the green body of the corresponding structure and use alcohol to clean it. Set the final temperature of the green body to 1450℃, the insulation time is 6h, and the detailed heating system is:

[0082] Stage 1) Room temperature—230°C, heating rate 0.5°C / min, holding time 1h, Ar atmosphere;

[0083] Stage 2) 230-290°C, heating rate 0.5°C / min, holding time 1h, Ar atmosphere;

[0084] Stage 3) 290-430°C, heating rate 0.5°C / min, holding time 1h, Ar atmosphere;

[0085] Stage 4) 430-500°C, heating rate 0.5°C / min, holding time 1h, Ar atmosphere;

[0086] Stage 5) 500-1450°C, heating rate 3°C / min, holding time 6h, Ar atmosphere;

[0087] Stage 6) Room temperature - 900 °C, heating rate 8 °C / min, holding time 24 h, air atmosphere;

[0088] The measured shrinkage of the green test sample after calcination was 16.24% in the X and Y axis directions and 18.96% in the Z axis direction. The model was enlarged according to the shrinkage of the X, Y and Z axes, and then the green formal sample was sintered according to the above sintering process to obtain the final printed part carrier. Figure 5 As shown, a SEM image of the printed part carrier obtained in Comparative Example 1 is provided.

[0089] Step 4: Same as Example 1.

[0090] Comparative Example 2:

[0091] Step 1 and step 2 are the same as in Example 1.

[0092] Step 3: Use the light-curing 3D printing equipment to print the green body of the corresponding structure and use alcohol to clean it. Set the final temperature of the green body to 1350℃, the insulation time is 6h, and the detailed heating system is:

[0093] Stage 1) Room temperature—230°C, heating rate 0.5°C / min, holding time 1h, air atmosphere;

[0094] Stage 2) 230-290, heating rate 0.5℃ / min, holding time 1h, air atmosphere;

[0095] Stage 3) 290-430, heating rate 0.5°C / min, holding time 1h, air atmosphere;

[0096] Stage 4) 430-500, heating rate 0.5°C / min, holding time 1h, air atmosphere;

[0097] Stage 5) 500-1350, heating rate 3°C / min, holding time 6h, air atmosphere;

[0098] The measured shrinkage of the green test sample after calcination was 22.11% in the X and Y axis directions and 25.48% in the Z axis direction. The model was enlarged according to the shrinkage of the X, Y and Z axes, and then the green formal sample was sintered according to the above sintering process to obtain the final printed part carrier. Figure 6 As shown, a SEM image of the printed part carrier obtained in Comparative Example 2 is provided.

[0099] Step 4: Same as Example 1.

[0100] Comparative Example 3:

[0101] Step 1: Same as Example 1

[0102] Step 2: Prepare 800g of nano-alumina, nano-magnesium oxide and nano-lanthanum oxide in a ratio of 14:1:4, add 1000ml of anhydrous ethanol and mix evenly, and use a planetary ball mill to mill the mixed powder at a speed of 400r / min for 6h and then dry. The dried solid is heated to 1450℃ in a muffle furnace at a heating rate of 53℃ / min, and kept warm for 6h to prepare a magnesium-based lanthanum hexaaluminate block. After the block is crushed, anhydrous ethanol is added to ball mill for 6h again. After ball milling, the powder is sieved through a 200 mesh sieve to obtain a powder raw material with a particle size of less than 75um. Take 500g of the powder raw material, add 112.5g of 4-hydroxybutyl acrylate, 1.25g of p-hydroxyphenyl ether, 5.625g of TPO, and 5.625g of polyethylene glycol, mix evenly and prepare a light-cured 3D printing slurry with a mass fraction of 75wt%.

[0103] Step 3: As in Example 1, the shrinkage of the green test sample after calcination was measured to be 4.35% in the X and Y axis directions and 7.17% in the Z axis direction. The model was enlarged according to the shrinkage of the X, Y and Z axes, and then the green formal sample was sintered according to the above sintering process to obtain the final printed part carrier. Figure 7 As shown, a SEM image of the printed part carrier obtained in Comparative Example 3 is provided.

[0104] Step 4: Same as Example 1.

[0105] like Figure 8 Shown are the N2O decomposition rate curves of the finished monolithic catalysts obtained in Example 1 and Comparative Examples 1 to 3.

[0106] Table 1 shows the experimental results of Example 1 and Comparative Examples 1-3.

[0107] Table 1 Experimental results of Example 1 and Comparative Examples 1 to 3

[0108]

[0109]

[0110] The technical features of the above embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0111] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a 3D printed monolithic catalyst, characterized in that: The following steps are involved: S1. Evenly mix the raw material powder of synthesized magnesium-based lanthanum hexaaluminate with a photocurable resin to obtain a 3D printing slurry; the photocurable resin comprises: a photocurable monomer, an inhibitor, a photoinitiator and a lubricant; S2, designing a three-dimensional model with a pore structure, importing the three-dimensional model into a 3D printer and performing slicing processing; S3, printing the 3D printing slurry into a monolithic catalyst green body of corresponding shape by the 3D printer, testing the TG-DSC curve of the monolithic catalyst green body, determining the sintering process of the monolithic catalyst green body in combination with the synthesis process of magnesium-based lanthanum hexaaluminate, and then calcining the monolithic catalyst green body according to the sintering process to obtain a monolithic catalyst carrier; the sintering process is: first sintering and carbonizing in an inert atmosphere, and then decarbonizing in an air atmosphere; S4, loading the monolithic catalyst carrier with active substances to obtain a monolithic catalyst.

2. The preparation method according to claim 1, characterized in that: In step S1, the photocurable monomer is one or more of 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, and dicyclopentenyl methacrylate, accounting for 60-90wt% of the mass fraction of the photocurable resin; The polymerization inhibitor is one or more of p-hydroxyphenyl ether, hydroquinone, tert-butyl catechol and copper naphthenate, accounting for 0.5-1wt% of the mass fraction of the photocurable resin; The photoinitiator is one or more of Irgacure 184, TPO, DMPA, and photoinitiator 819, accounting for 3-10wt% of the mass fraction of the photocurable resin; The lubricant is one or more of polyethylene glycol, oleic acid, stearic acid, and trioctylphosphine oxide, accounting for 1-10wt% of the mass fraction of the photocurable resin; After the photocurable resin and the raw material powder are mixed into a 3D printing slurry, the raw material powder accounts for 50-55wt% of the 3D printing slurry.

3. The preparation method according to claim 1, characterized in that: The preparation process of the raw material powder for synthesizing magnesium-based lanthanum hexaaluminate in step S1 is as follows: Weigh a certain mass ratio of nano-alumina powder, nano-magnesium oxide powder and nano-lanthanum oxide powder, add a certain proportion of defoaming agent and adhesive, add an appropriate amount of dispersant to dissolve, mechanically stir evenly to obtain a solution suitable for spray drying granulation, then perform centrifugal spray drying granulation, sieve, and prepare a raw material mixed powder with a suitable particle size. Among them, the particle sizes of nano-alumina powder, nano-magnesium oxide powder and nano-lanthanum oxide powder are all 40-50nm; The particle size U90% of the raw material mixed powder after spray drying, granulation and sieving is 1-10 μm, and the maximum particle size does not exceed 75 μm.

4. The preparation method according to claim 3, characterized in that: In step S1, the mass ratio of nano-alumina powder, nano-magnesium oxide powder and nano-lanthanum oxide powder is (13-14):1:(4-4.5).

5. The preparation method according to claim 3, characterized in that: In step S1, the mass proportion of the defoaming agent is 0.5-1.0% of the total mass of the nano-alumina powder, the nano-magnesium oxide powder and the nano-lanthanum oxide powder; The mass proportion of the binder is 1-3% of the total mass of the nano-alumina powder, the nano-magnesia powder and the nano-lanthanum oxide powder; In the solution suitable for spray drying granulation, the mass ratio of the total mass of the nano-alumina powder, the nano-magnesium oxide powder and the nano-lanthanum oxide powder to the mass of the dispersant is 1:(3-5).

6. The preparation method according to claim 3, characterized in that: In step S1, the defoaming agent is one or more of triammonium citrate, polydimethylsilane, and tributyl phosphate; The binder is one or more of gum arabic, ethyl cellulose and povidone; The dispersant is one or more of water and anhydrous ethanol.

7. The preparation method according to claim 1, characterized in that: In step S3, the sintering process is as follows: Carbonization sintering in inert atmosphere: 1) From room temperature to 220-240℃, the heating rate is 0.4-0.6℃ / min, and the insulation time is 1-2h; 2) From 220-240℃ to 280-300℃, the heating rate is 0.4-0.6℃ / min, and the insulation time is 1-2h; 3) From 280-300℃ to 420-440℃, the heating rate is 0.4-0.6℃ / min, and the insulation time is 1-2h; 4) From 420-440℃ to 480-500℃, the heating rate is 0.4-0.6℃ / min, and the insulation time is 1-2h; 5) From 480-500℃ to 1300-1400℃, the heating rate is 2-4℃ / min, and the insulation time is 4-8h; Carbon removal in air atmosphere: 6) From room temperature to 800-1000℃, the heating rate is 5-10℃ / min, and the insulation time is 20-28h.

8. The preparation method according to claim 1, characterized in that: Step S4 specifically includes: The monolithic catalyst carrier is immersed in a 5-10% by mass liquid chloroiridic acid, and after immersion for 30-40 minutes, it is taken out and dried in an oven at above 80° C. for 30-60 minutes until the surface is completely dry; Then roast at 400-450°C in air atmosphere, keep warm for 1-2 hours, and repeat oxidation roasting 5-10 times; Then, the product is reduced at 300-350° C. in a hydrogen atmosphere for 1-2 hours to obtain the final finished monolithic catalyst.

9. A 3D printed monolithic catalyst, characterized in that: The method is prepared according to claim 1-8.

10. An application of a 3D printed monolithic catalyst, characterized in that: The 3D printed monolithic catalyst as described in claim 9 or the 3D printed monolithic catalyst prepared by the preparation method as described in claims 1-8 is applied to the decomposition of liquid propellant N2O.

Citation Information

Patent Citations

  • Catalyst and preparation and application thereof

    CN101927160A

  • Preparation method of structuralized Ni-alumina / carbon catalyst through assistance of 3D printing technique

    CN107442127A

  • Supported noble metal catalysts with performance of resisting high-temperature sintering and preparing method thereof

    CN108452809A

  • Preparation method of spherical magnesium-based lanthanum hexaaluminate spray powder

    CN109160811A

  • Monolithic catalyst based on 3D printing, preparation method and application

    CN115282973A

Cited By

  • Monolithic catalyst and granular catalyst equivalent test method and device

    CN119470764A

  • Method for preparing fine-grain tough oral all-ceramic material by interface inhibition method and application of fine-grain tough oral all-ceramic material

    CN122277247A