Cu-ZnO coated Al2O3 catalyst as well as preparation method and application thereof

By preparing the Cu-ZnO@Al2O3 catalyst, the low selectivity of furfural electrocatalytic hydrogenation reaction and the Cu catalyst current attenuation were solved, and the high selectivity and stable furfural electroreduction performance were achieved, and the selectivity of 2-methylfuran was generated. 95%.

CN118874552AActive Publication Date: 2024-11-01CHONGQING UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411005841.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-01
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The selectivity of furfural electrocatalytic hydrogenation reaction is not high, and the current decays too fast when using Cu catalyst alone, resulting in low Faraday efficiency.

Method used

Using Cu-ZnO@Al2O3 catalyst, the copper salt, zinc salt and aluminum salt are dissolved in water, adjusted the pH value and precipitated, dried and calcined, and finally calcined in a reducing atmosphere to prepare a polyL acid site. Cu-ZnO@Al2O3 catalyst, used for electrical reduction of furfural.

Benefits of technology

The C-O bond fracture selectivity during furfural electrocatalytic hydrogenation process is significantly improved, and the selectivity of 2-methylfuran is reached 95%, avoiding the rapid inactivation of the elemental Cu cathode electrode material and the steep current drop.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874552A_ABST
    Figure CN118874552A_ABST
Patent Text Reader

Abstract

The invention discloses a Cu-ZnO-coated Al2O3 catalyst as well as a preparation method and application thereof, and belongs to the technical field of catalyst preparation. The Cu-ZnO-coated Al2O3 catalyst is prepared by using a coprecipitation method and a calcination reduction method, and oxides of Zn and Al are introduced on the basis of taking Cu as an active component, so that the Cu-ZnO-coated Al2O3 catalyst presents more L acid sites, thereby promoting C-O bond breakage in the furfural electro-catalytic hydrogenation process, and improving the yield of the furfural electro-catalytic hydrogenation catalyst. And finally, the excellent catalytic performance of generating 2-methylfuran through furfural electroreduction in a high-selectivity mode is obtained, the selectivity of 2-methylfuran is 95% after the reaction is carried out for 1 h at the constant voltage of-0.5 V vs.SHE, and meanwhile the problems that elemental Cu serving as a cathode electrode material is rapidly inactivated and the current drops suddenly are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst preparation, and specifically relates to a Cu-ZnO@Al2O3 catalyst and a preparation method and application thereof. Background Art

[0002] Furfural is a key product in the biorefining industry, and value-added products derived from furfural (such as 2-methylfuran) are widely used in the chemical and energy industries. Traditional methods for reducing furfural are hydrodeoxygenation and catalytic hydrogen transfer, but both have some disadvantages, such as the use of high-pressure hydrogen, toxic reducing agents, or high-temperature reaction conditions during the reduction process. Electrochemical hydrogenation provides a sustainable reduction method for reducing furfural to 2-methylfuran. In the electrochemical reduction process, the hydrogen source comes from water or protons in the solution, and renewable energy electricity can be used to convert water or protons in the solution into adsorbed hydrogen. The adsorbed hydrogen is adsorbed on the electrode surface to further carry out the furfural hydrogenation reaction under mild reaction conditions. However, due to the competition of side reactions in the electrochemical hydrogenation of furfural, the electrochemical reduction method to obtain 2-methylfuran still has problems such as low activity and low Faraday efficiency.

[0003] A series of catalysts have been developed for the electrocatalytic hydrogenation reaction of furfural, such as Cu, Pb, Fe, Pt, Pd, Ti and graphite. Among them, Cu is the most promising because it is non-precious metal and has high selectivity. However, when Cu is used alone as a catalyst, the current decays too quickly, resulting in a low conversion rate Faraday efficiency. In the prior art, a series of CuPd catalysts are used to electrochemically hydrogenate furfural to 2-methylfuran in 0.1M acetic acid aqueous solution (pH=2.9). At -0.58V vs RHE, the highest Faraday efficiency (FE) of 2-methylfuran reaches 75%, but the current density is only -4.5mA / cm 2 , the reaction current is too small. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a Cu-ZnO@Al2O3 catalyst and a preparation method and application thereof, so as to solve the technical problem that the selectivity of furfural electroreduction is not high.

[0005] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing a Cu-ZnO@Al2O3 catalyst, comprising the following steps:

[0006] S1. Dissolve copper salt, zinc salt and aluminum salt in water to obtain a mixed solution, then add the mixed solution to a carbonate solution at 35-45°C, adjust the pH value of the reaction system to 9-10, and finally heat to 55-85°C for 12-24h, centrifuge to obtain a precipitate; the molar ratio of Cu, Zn and Al ions in the mixed solution is 2-6:1-3:1-3;

[0007] S2. Dry the precipitate at 60-100°C for 12-48h, then heat it to 500-900°C and calcine it for 2-8h. Finally, place the calcined sample in a reducing atmosphere and reduce it at 500-900°C for 2-6h to obtain a Cu-ZnO@Al2O3 catalyst.

[0008] On the basis of the above technical solution, the present invention can also be improved as follows:

[0009] Furthermore, the copper salt is copper nitrate, copper sulfate or copper chloride, the zinc salt is zinc nitrate, zinc sulfate or zinc chloride, and the aluminum salt is aluminum nitrate, aluminum sulfate or aluminum chloride.

[0010] Furthermore, the carbonate solution is a sodium carbonate or potassium carbonate solution.

[0011] Furthermore, the reagent for adjusting the pH value of the reaction system is NaOH or KOH solution.

[0012] Furthermore, the reaction temperature in S1 is 70° C. and the reaction time is 18 h.

[0013] Furthermore, S2 also includes washing the precipitate to neutrality before drying.

[0014] Furthermore, the calcination temperature in S2 is 500°C, and the calcination time is 4 hours; the reduction temperature is 500°C, and the reduction time is 2 hours.

[0015] Furthermore, the gases used in the reducing atmosphere are H2 and N2.

[0016] Further, the flow rate of H2 is 5-15 mL / min, and the flow rate of N2 is 85-95 mL / min.

[0017] The invention also discloses a Cu-ZnO@Al2O3 catalyst prepared by the preparation method.

[0018] The invention also discloses the application of Cu-ZnO@Al2O3 catalyst in furfural reduction.

[0019] The beneficial effects of the present invention are as follows: the Cu-ZnO@Al2O3 catalyst prepared by the present invention has a large number of L acid sites, thereby promoting the cleavage of the CO bond during the electrocatalytic hydrogenation of furfural, and finally obtaining a relatively excellent catalytic performance of furfural electroreduction with high selectivity to generate 2-methylfuran. The use of acidic oxides such as Al2O3, ZSM-5 and SiO2 as carriers can improve the selectivity of Cu-ZnO catalytic furfural hydrogenation to generate 2-methylfuran, and exhibits efficient furfural electroreduction to generate 2-methylfuran in a 0.5M H2SO4 solution. At a constant voltage reaction of -0.5V vs. SHE for 1h, the selectivity of 2-methylfuran is 95%, and the problem of rapid deactivation and steep current drop of single substance Cu as a cathode electrode material is avoided. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 is the XRD pattern of Cu;

[0021] Figure 2 is the XRD pattern of ZnO;

[0022] Figure 3 is the XRD pattern of Cu-ZnO;

[0023] Figure 4 This is the XRD spectrum of Cu-ZnO@Al2O3.

[0024] Figure 5 This is the high-resolution XPS spectrum of Zn in Cu-ZnO@Al2O3;

[0025] Figure 6 This is the high-resolution XPS spectrum of Cu in Cu-ZnO@Al2O3;

[0026] Figure 7 This is the high-resolution XPS spectrum of Al in Cu-ZnO@Al2O3;

[0027] Figure 8 The morphological characteristics of Cu-ZnO@Al2O3; wherein, Figure (a) is a TEM image at 50nm, Figure (b) is a TEM image at 10nm, Figure (c) is a mapping scan of Cu-ZnO@Al2O3, Figure (d) is a mapping scan of the O element, Figure (e) is a mapping scan of the Al element, Figure (f) is a mapping scan of the Cu element, and Figure (g) is a mapping scan of the Zn element;

[0028] Fig. 9 The effect of aluminum nitrate concentration on the furfural conversion and 2-methylfuran Faraday efficiency of Cu-ZnO@Al2O3 catalyst;

[0029] Fig.10 The effect of aluminum nitrate concentration on the selectivity of furfural reduction products over Cu-ZnO@Al2O3 catalyst;

[0030] Fig.11 XRD patterns of Cu-ZnO@Al2O3 catalysts prepared at different zinc nitrate concentrations;

[0031] Fig.12 The effect of zinc nitrate concentration on the furfural conversion and 2-methylfuran Faraday efficiency of Cu-ZnO@Al2O3 catalyst;

[0032] Fig.13 The effect of zinc nitrate concentration on the selectivity of furfural reduction products over Cu-ZnO@Al2O3 catalyst;

[0033] Fig.14 NH3-TPD spectra of Cu and Cu-ZnO@Al2O3 catalysts;

[0034] Fig.15 The product selectivity of materials prepared based on different acidic oxides;

[0035] Fig.16 LSV curves of Cu-ZnO@Al2O3 and Cu and Zn metal sheets before and after adding furfural;

[0036] Fig.17 The product selectivity of Cu-ZnO@Al2O3 and Cu and Zn metal sheets;

[0037] Fig.18 It is the constant voltage reaction curve of Cu-ZnO@Al2O3 and Cu metal sheet;

[0038] Fig.19 LSV curves of Cu-ZnO@Al2O3 and Cu, ZnO and Al2O3 powders before and after adding furfural;

[0039] Fig. 20 The product selectivity of Cu-ZnO@Al2O3 and Cu, ZnO and Al2O3 powders. DETAILED DESCRIPTION

[0040] The specific embodiments of the present invention are described below to facilitate the understanding of the present invention by those skilled in the art. If the specific conditions are not specified in the examples, the methods are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturers are not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially. However, it should be clear that the present invention is not limited to the scope of the specific embodiments. For those skilled in the art, as long as various changes are within the spirit and scope of the present invention defined and determined by the attached claims, these changes are obvious, and all inventions and creations using the concept of the present invention are protected.

[0041] Example 1

[0042] A method for preparing a Cu-ZnO@Al2O3 catalyst comprises the following steps:

[0043] S1. Dissolve 12.1245 g Cu(NO3)2·3H2O, 7.43725 g Zn(NO3)2·6H2O and 9.37825 g Al(NO3)3·9H2O in 100 mL water to obtain a mixed solution (0.5 M Cu(NO3)2·3H2O, 0.25 M Zn(NO3)2·6H2O and 0.25 M Al(NO3)3·9H2O). Then add the mixed solution into a 100 mL sodium carbonate solution with a concentration of 0.125 M at 40°C to make Cu(NO3)2·3H2O. 2+ 、Zn 2+ 、Al 3+ It was converted into carbonate precipitate, and the pH value of the reaction system was adjusted to 9.5 with a 1M NaOH solution to form a layered structure. Finally, the temperature was raised to 70°C and reacted for 18 hours, and centrifuged to obtain a precipitate.

[0044] S2. Wash the precipitate with ethanol and deionized water until it is neutral, then dry the precipitate at 80°C for 30 hours, then heat it to 500°C and calcine it for 4 hours. Finally, place the calcined sample in a reducing atmosphere (a mixed atmosphere of H2 and N2, with a flow rate of H2 of 10 mL / min and a flow rate of N2 of 90 mL / min) and reduce it at 500°C for 2 hours to obtain a Cu-ZnO@Al2O3 catalyst.

[0045] Example 2

[0046] A method for preparing a Cu-ZnO@Al2O3 catalyst comprises the following steps:

[0047] S1. Dissolve 12g CuSO4·3H2O, 7g ZnSO4·6H2O and 9g Al2(SO4)3·9H2O in 100mL water to obtain a mixed solution. Then add the mixed solution into a 0.125M sodium carbonate solution with a volume of 100mL at 35°C to make CuSO4·3H2O and ZnSO4·6H2O. 2 + 、Zn 2+ 、Al 3+ The mixture was converted into carbonate precipitate, and the pH value of the reaction system was adjusted to 10 with a 1M NaOH solution to form a layered structure. The mixture was heated to 55°C and reacted for 24 hours. The mixture was centrifuged to obtain a precipitate.

[0048] S2. Wash the precipitate with ethanol and deionized water until it is neutral, then dry the precipitate at 100°C for 12 hours, then heat it to 700°C and calcine it for 8 hours. Finally, place the calcined sample in a reducing atmosphere (a mixed atmosphere of H2 and N2, with a flow rate of H2 of 5 mL / min and a flow rate of N2 of 95 mL / min) and reduce it at 700°C for 4 hours to obtain a Cu-ZnO@Al2O3 catalyst.

[0049] Example 3

[0050] A method for preparing a Cu-ZnO@Al2O3 catalyst comprises the following steps:

[0051] S1. Dissolve 13g CuCl2·3H2O, 7g ZnCl2·6H2O and 9g AlCl3·9H2O in 100mL water to obtain a mixed solution. Then add the mixed solution into a 0.125M potassium carbonate solution with a volume of 100mL at 45°C to make CuCl2·3H2O and ZnCl2·6H2O. 2+ 、Zn 2+ 、Al 3+ It was converted into carbonate precipitate, and the pH value of the reaction system was adjusted to 9 with a 1M KOH solution to form a layered structure. Finally, the temperature was raised to 85°C and reacted for 12 hours, and centrifuged to obtain a precipitate.

[0052] S2. Wash the precipitate with ethanol and deionized water until it is neutral, then dry the precipitate at 60°C for 48 hours, then heat it to 900°C and calcine it for 2 hours. Finally, place the calcined sample in a reducing atmosphere (a mixed atmosphere of H2 and N2, with a flow rate of H2 of 15 mL / min and a flow rate of N2 of 85 mL / min) and reduce it at 900°C for 2 hours to obtain a Cu-ZnO@Al2O3 catalyst.

[0053] Comparative Example 1

[0054] The difference between this comparative example and Example 1 is that Zn(NO3)2·6H2O and Al(NO3)3·9H2O in step S1 are omitted, and the remaining components are the same as the preparation method and Example 1 to obtain a Cu catalyst.

[0055] Comparative Example 2

[0056] The difference between this comparative example and Example 1 is that Cu(NO3)2·3H2O and Al(NO3)3·9H2O in step S1 are omitted, and the remaining components are the same as the preparation method and Example 1 to obtain a ZnO catalyst.

[0057] Comparative Example 3

[0058] The difference between this comparative example and Example 1 is that Al(NO3)3·9H2O in step S1 is omitted, and the remaining components are the same as the preparation method and Example 1 to obtain a Cu-ZnO catalyst.

[0059] Experimental Example 1 Structural Characterization

[0060] 1.XRD test

[0061] The catalyst samples prepared in Example 1 and Comparative Examples 1-3 were subjected to XRD testing to analyze the component information and crystal structure of the catalysts. The results are as follows: Figure 1-Figure 4 shown.

[0062] like Figure 1 As shown in Figure 4, the XRD diffraction peaks at 43.3°, 50.4°, 74.1°, and 89.9° correspond to the (1 1 1), (2 0 0), (2 2 0), and (3 1 1) crystal planes of elemental Cu, respectively (PDF#4-836). Figure 4 As shown in the figure, the diffraction peaks at positions of 31.7°, 34.4°, 36.2°, and 47.5° correspond to the (1 0 0), (0 0 2), (1 0 1), and (1 0 2) crystal planes of ZnO and the diffraction peaks of Al2O3, and compared with the standard card (PDF#10-0425), it is found that the Al2O3 in the catalyst prepared in Example 1 is γ phase. It can be seen that Cu in Cu-ZnO@Al2O3 exists in the form of a single substance, while Zn and Al exist in the form of oxides.

[0063] 2.XPS test

[0064] XPS tests were performed to investigate the elemental composition and chemical state of the Cu-ZnO@Al2O3 catalyst surface. Figure 5 ) It can be seen that the peaks at 1044.8eV and 1022.1eV are similar to those at Zn 2+ Related, combined with the XRD spectrum of Cu-ZnO@Al2O3 ( Figure 4 ) can indicate that during the preparation process, Zn oxide is not reduced because it has not reached its reduction temperature, so zinc exists in the form of ZnO. Figure 6 This is the XPS spectrum of the Cu element. In addition to the characteristic peaks of CuO, two significant Cu 2+ Satellite peaks may be caused by oxidation of the Cu surface during the test. Figure 7 ) It can be seen that Al exists in the form of Al 3+ This is also because the reduction temperature during the preparation process did not reach the reduction temperature of Al2O3 (900℃).

[0065] 3.TEM test

[0066] The surface structure and morphology of Cu-ZnO@Al2O3 catalyst were characterized by transmission electron microscopy (TEM). Figure 8 As shown. Figure 8 (a) It can be seen that the Cu-ZnO@Al2O3 catalyst exhibits a nanosheet structure; Figure 8 (b) shows lattice fringes with spacing of 0.288 nm and 0.278 nm, which correspond to the ZnO (1 1 0) crystal plane and the Al2O3 (22 2) crystal plane, respectively.

[0067] The element distribution of Cu-ZnO@Al2O3 catalyst was further studied by mapping scanning, such as Figure 8 (c)- Figure 8 As shown in (g), the distribution of elements is relatively uniform.

[0068] Experimental Example 2 Optimization of catalyst preparation conditions

[0069] Taking the preparation process of Example 1 as an example, the following experiment was carried out:

[0070] 1. Aluminum nitrate concentration

[0071] With other conditions unchanged, the concentration of aluminum nitrate was changed (0.125M, 0.25M, 0.375M and 0.5M) to prepare a series of Cu-ZnO@Al2O3 catalysts with different aluminum contents. Fig. 9 and Fig.10 As shown in the figure, when the amount of added Al2O3 increases, the furfural conversion rate, 2-methylfuran selectivity and Faraday efficiency all increase first and then decrease, and the relevant performance reaches the maximum value when the aluminum nitrate concentration is 0.25 M. This is because the conductivity of Al2O3 is poor. When there is too much Al2O3, the conductivity of the catalyst deteriorates, which affects the furfural conversion and the formation of 2-methylfuran.

[0072] 2. Concentration of zinc nitrate

[0073] The effect of ZnO on the reduction activity of furfural was investigated by introducing different amounts of ZnO. The introduction of ZnO can increase the L-acid concentration of Al2O3. At the same time, the presence of Zn will inhibit the sintering of metal particles and act as a dispersant for other metal substances. Under the condition that other conditions remain unchanged, the concentration of zinc nitrate is changed (0M, 0.125M, 0.25M, 0.5M and 1M) to prepare a series of Cu-ZnO@Al2O3 catalysts with different ZnO contents. The results are shown in Figure 2. Fig.11 As shown, with the increase of zinc nitrate concentration, the peak intensity of ZnO becomes higher and higher, and the crystallinity becomes higher and higher, that is, the proportion of zinc oxide in the catalyst increases. Fig.12 and Fig.13 It shows that the optimal concentration of zinc nitrate is 0.25M. When the concentration is too high, the furfural conversion rate drops sharply. This is because the addition of too much ZnO reduces the number of active sites and the conductivity of the catalyst, resulting in a decrease in the reduction current of furfural.

[0074] Experimental Example 3 Catalyst Activity Analysis

[0075] In order to explore the mechanism of ZnO and Al2O3 on the performance improvement of Cu-ZnO@Al2O3 catalyst, this experimental example conducted NH3-TPD test on Cu-ZnO@Al2O3 material. Fig.14 As shown, it is obvious that the Cu powder alone is not acidic, but after adding ZnO and Al2O3, the Cu-ZnO@Al2O3 material shows strong acidity.

[0076] Using commercial Al2O3, ZSM-5 (silicon aluminum molecular sieve) and SiO2 three acidic oxide powders as substrates, the aluminum salt in Example 1 was replaced with different acidic oxide powders to prepare Cu-ZnO / Al2O3, Cu-ZnO / ZSM-5, and Cu-ZnO / SiO2 catalysts. The catalyst was used as the cathode and constant voltage electrolysis was performed at -0.5V vs. SHE voltage. The product distribution results are as follows Fig.15 As shown. It can be seen that although the catalytic activity of the catalysts prepared with three different substrates (Cu-ZnO / Al2O3, Cu-ZnO / ZSM-5 and Cu-ZnO / SiO2) is not as good as the Cu-ZnO@Al2O3 catalyst prepared in Example 1, the selectivity of 2-methylfuran is significantly improved in the catalysts with three acidic substrates of Al2O3, ZSM-5 and SiO2 compared with the Cu-ZnO catalyst without acidic oxide. It can be seen that improving the acidity of the catalyst is helpful to improve the selectivity of 2-methylfuran.

[0077] Experimental Example 4 Furfural electroreduction performance test

[0078] The furfural electroreduction performance was tested using a three-electrode system (working electrode, counter electrode and reference electrode) in an H-type electrolyzer with a proton membrane separating the anode and cathode. The working electrode was the sample to be tested, and the electrode working area was 1 cm × 1 cm. The counter electrode was a shape-stable anode DSA with an area of ​​2 cm × 2 cm. The reference electrode was Ag / AgCl. The anode and cathode were both 30 mL, 0.5 M H2SO4 electrolyte solution, the concentration of furfural in the cathode reaction organic matter is 20mM. With the standard hydrogen electrode (SHE) as a reference, all experiments were carried out at 40°C, CV test was carried out at 100mv / s, and LSV test was carried out at 5mv / s. The H-type electrolyzer is connected to a Monte Carlo wash bottle filled with 30mL acetonitrile as a 2-methylfuran collector, and the exhaust gas treatment device is connected after the collector. N2 is used as a purge gas throughout the reaction. The target product 2-methylfuran is collected by the collector, and after adding the internal standard, it is detected by gas chromatography, while the raw material furfural and the by-product furfuryl alcohol are detected by high performance liquid chromatography.

[0079] The furfural reduction activity of Zn, Cu electrode sheets, blank carbon paper and Cu-ZnO@Al2O3 catalysts was compared. In the electrolyte without furfural, the cathodic polarization curve was attributed to the hydrogen evolution reaction. Fig.16 As shown in the figure, as the electrode potential moves negatively, the HER activity of Cu metal sheet becomes more and more advantageous compared with Cu-ZnO@Al2O3. When 20 mM furfural is added to the electrolyte, the electroreduction materials on the cathodes of all materials move positively, indicating that the furfural reduction reaction on all electrode materials is faster than the hydrogen evolution reaction. Although the hydrogen evolution activity of Cu is basically better than that of Cu-ZnO@Al2O3 catalyst in the entire test voltage range, after the addition of furfural, the Cu-ZnO@Al2O3 cathode shows a significant increase in current density in the same scanning potential range, that is, the furfural reduction activity is more improved, and in the range of -0.2 to -0.5 V vs. SHE, the furfural reduction activity of Cu-ZnO@Al2O3 is better than that of Cu metal sheet.

[0080] The reaction was carried out at a constant potential of -0.5 V vs SHE for 1 h to investigate the performance of furfural conversion, selectivity and Faraday efficiency when Cu-ZnO@Al2O3 and Cu and Zn metal sheets were used as cathode electrodes. Fig.17 As shown in the figure, furfural is converted to 2-methylfuran with the highest selectivity (95%). Although the highest selectivity of the Cu metal sheet can reach more than 90%, the current decay is too fast on the Cu metal sheet, while the current stability of the Cu-ZnO@Al2O3 catalyst has been significantly improved ( Fig.18 ), avoiding the problem of rapid deactivation and steep current drop of single-element Cu as cathode electrode material.

[0081] By comparing the performance of furfural electroreduction reaction of catalysts with different compositions, the results are as follows Fig.19 and Fig. 20 As shown. Fig.19 It was observed that when no organic matter was added, the hydrogen evolution activity of Cu / CP was higher than that of Cu-ZnO@Al2O3 catalyst. However, after adding 20 mM furfural, the current density of Cu-ZnO@Al2O3 was higher than that of Cu / CP in the voltage range of -0.2 to 0.5 V vs SHE. Fig. 20 It can be seen that the selectivity of the product 2-methylfuran after constant potential electrolysis is ranked as Cu

Claims

1. A method for preparing a Cu-ZnO@Al2O3 catalyst, characterized in that: The following steps are involved: S1. Dissolve copper salt, zinc salt and aluminum salt in water to obtain a mixed solution, then add the mixed solution to a carbonate solution at 35-45°C, adjust the pH value of the reaction system to 9-10, and finally heat to 55-85°C for 12-24h, centrifuge to obtain a precipitate; the molar ratio of Cu, Zn and Al ions in the mixed solution is 2-6:1-3:1-3; S2. Dry the precipitate at 60-100°C for 12-48h, then heat it to 500-900°C and calcine it for 2-8h. Finally, place the calcined sample in a reducing atmosphere and reduce it at 500-900°C for 2-6h to obtain a Cu-ZnO@Al2O3 catalyst.

2. The method for preparing the Cu-ZnO@Al2O3 catalyst according to claim 1, characterized in that: The copper salt is copper nitrate, copper sulfate or copper chloride, the zinc salt is zinc nitrate, zinc sulfate or zinc chloride, and the aluminum salt is aluminum nitrate, aluminum sulfate or aluminum chloride.

3. The method for preparing the Cu-ZnO@Al2O3 catalyst according to claim 1, characterized in that: The reagent for adjusting the pH value of the reaction system is NaOH or KOH solution.

4. The method for preparing the Cu-ZnO@Al2O3 catalyst according to claim 1, characterized in that: The reaction temperature in S1 is 70° C. and the reaction time is 18 h.

5. The method for preparing the Cu-ZnO@Al2O3 catalyst according to claim 1, characterized in that: The S2 also includes washing the precipitate to neutrality before drying.

6. The method for preparing the Cu-ZnO@Al2O3 catalyst according to claim 1, characterized in that: The calcination temperature in S2 is 500° C. and the calcination time is 4 h; the reduction temperature is 500° C. and the reduction time is 2 h.

7. The method for preparing the Cu-ZnO@Al2O3 catalyst according to claim 1, characterized in that: The gases used in the reducing atmosphere are H2 and N2.

8. The method for preparing the Cu-ZnO@Al2O3 catalyst according to claim 7, characterized in that: The flow rate of H2 is 5-15 mL / min, and the flow rate of N2 is 85-95 mL / min.

9. A Cu-ZnO@Al2O3 catalyst, characterized in that: The method is prepared by the method according to any one of claims 1 to 8.

10. Use of the Cu-ZnO@Al2O3 catalyst according to claim 9 in furfural reduction.

Citation Information

Patent Citations

  • 2-methyl furan catalyst and preparation method thereof

    CN104383929A

  • Catalyst used for preparing 2,5-methyl furan and preparation method thereof

    CN105435800A

  • Copper-based catalyst as well as preparation method and application thereof

    CN113430545A

  • Catalyst for preparing p-xylene through hydrogenation of waste PET, and preparation method and application thereof

    CN116393139A

  • Method for electrolytically converting organic compounds

    US6733652B1