Supersaturated silver-bismuth solid solution nano-particles, preparation method thereof and application of nano-particles in sintering slurry

Supersaturated silver bismuth solid solution nanoparticles were prepared by low-temperature in-situ chemical synthesis. Combined with sintering slurry technology, the problem of high sintering temperature of nanosilver and copper slurry was solved, low-temperature sintering below 180℃ was achieved, and welding points were improved Thermal conductivity and reliability are suitable for devices with poor heat resistance and gradient interconnect applications.

CN118875307AActive Publication Date: 2024-11-01HARBIN INST OF TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410921027.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-01
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

The existing nanosilver and copper slurries have high sintering temperatures, making it difficult to sinter at low temperatures below 180°C, which affects the reliability and heat resistance of the solder joints, is easy to oxidize, and has poor storage performance.

Method used

The low-temperature in-situ chemical synthesis method is adopted to form supersaturated silver bismuth solid solution nanoparticles by selecting suitable solvents and strong reducing agents, and prepare sintered slurry with organic solutions, dispersants, fluxes and binders, and perform hot pressure at low temperatures. Sintering, bismuth element exists stably at the nanometer size, reducing the sintering temperature.

Benefits of technology

It realizes low-temperature sintering below 180°C, reduces internal thermal stress of solder joints, improves thermal conductivity and reliability of solder joints, and reduces costs. It is suitable for devices with poor heat resistance and gradient interconnection applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875307A_ABST
    Figure CN118875307A_ABST
Patent Text Reader

Abstract

The invention discloses a supersaturated silver-bismuth solid solution nanoparticle, a preparation method thereof and application of the supersaturated silver-bismuth solid solution nanoparticle in sintering slurry, and belongs to the technical field of sintering materials and preparation of the sintering materials. The problem of high sintering temperature in the existing nano slurry is solved. According to the preparation method, a low-temperature in-situ chemical synthesis method is adopted, a strong reducing agent is used for achieving liquid-phase rapid unsteady-state reaction, silver and bismuth ions are rapidly reduced synchronously in situ, metal is rapidly nucleated and grown in the liquid phase, bismuth atoms are neatly arranged in a silver metal face-centered cubic lattice under the influence of an unsteady-state reaction mechanism, and the silver-bismuth composite material is obtained. And a silver lattice silver-bismuth binary single-phase supersaturated solid solution which is unstable but stably exists is formed. Nanometer slurry prepared from the solid solution can be sintered at the temperature of 180 DEG C or even lower ultralow temperature, the requirement for the sintering process is low, the nanometer slurry can be sintered in air, the shear strength of a sintered welding spot is 12-40 MPa, and the heat conductivity is 100-300 W / (m.K).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to supersaturated silver-bismuth solid solution nanoparticles and a preparation method thereof and application thereof in sintering slurry, belonging to the technical field of sintering materials and preparation thereof. Background Art

[0002] As the third-generation semiconductors, led by gallium nitride (GaN) and silicon carbide (SiC), are gradually applied to power devices such as RF devices, power devices, high-power LED devices, insulated gate bipolar transistors (IGBTs) and laser modules. The high breakdown voltage and wide bandgap characteristics of the third-generation semiconductors determine the high withstand voltage characteristics of the power device; and the high thermal conductivity and high heat resistance characteristics enable the device to withstand higher junction temperatures. In addition, the working environment of power devices mainly used in automotive electronics, high-voltage power transmission, and charging equipment is also relatively harsh, and they usually have to work in high temperature and exposure environments. These characteristics determine that the service temperature of the third-generation semiconductor devices is much higher than that of traditional silicon-based power devices. Its service temperature is often higher than 200°C, and even the peak temperature is as high as 600°C, which puts extremely stringent heat resistance and heat dissipation requirements on the device package. The solder joints in the existing package often use tin-based solder as the connection material, and the excessively high service temperature will cause the solder joints to degrade rapidly, and even occasionally exceed the melting point of the solder, causing device failure.

[0003] Existing research results show that nano-pastes based on nano-silver are undoubtedly the best alternative to traditional solders. This material can be sintered at low temperatures and its thermal conductivity can reach 3-4 times that of traditional tin-based solders. However, the sintering temperature of nano-silver paste is difficult to be lower than 200°C, and the nano-copper paste that has been vigorously developed in recent years even needs to be sintered at more than 250°C, and the application of nano-pastes often requires lower sintering temperatures. For example, higher sintering temperatures will lead to higher thermal stress inside the solder joints, affecting the reliability of the solder joints. Some devices require gradient interconnection, so sintering materials below 200°C are required. In addition to power devices, some devices with poor heat resistance also require high thermal conductivity of the package body, and the sintering temperature of nano-silver and copper limits their application in these areas. For unit metal nano-pastes, it is difficult to further reduce the sintering temperature through process means, and nano-scale low-melting-point metals are generally easy to oxidize, have poor storage performance and are difficult to sinter.

[0004] In recent years, based on unit nanometal slurries, researchers have developed a few nanoslurries with binary or even multinary alloy nanoparticles as solid phase components, including different types of multinary alloys such as copper-silver, copper-tin, and silver-aluminum. Among them, copper-silver alloys have been the most studied, including copper-silver core-shell nanoparticles, copper-silver solid solution nanoparticles, etc. The main advantages of this type of material include resistance to electromigration, corrosion resistance, and low cost. However, due to the high melting point of copper metal, the sintering temperature is higher than that of nanosilver. In addition, copper-tin compound alloy nanoparticles also have the problem of high sintering temperature. Therefore, in order to achieve the purpose of lowering the sintering temperature, it is necessary to add low-melting-point metals on the basis of nanosilver to meet the sintering temperature at 180°C or even lower. Summary of the invention

[0005] Aiming at the problem of high sintering temperature in existing nano slurry, the present invention provides a supersaturated silver-bismuth solid solution nano particle and a preparation method thereof and application in sintering slurry.

[0006] The technical solution of the present invention:

[0007] One of the purposes of the present invention is to provide a method for preparing supersaturated silver-bismuth solid solution nanoparticles, the method comprising the following steps:

[0008] (1) placing a silver metal salt and a bismuth metal salt in a reaction container in proportion, adding an organic dispersant and a solvent, and stirring until completely dissolved to obtain a precursor solution;

[0009] (2) The precursor solution and the reducing agent solution are mixed and reacted under low temperature conditions to obtain silver-bismuth solid solution nanoparticles.

[0010] It is further defined that the silver metal salt in (1) is a mixture of one or more of silver nitrate, silver sulfate, silver oxalate, silver chloride, silver bromide and silver iodide.

[0011] It is further defined that the bismuth metal salt in (1) is a mixture of one or more of bismuth nitrate, bismuth chloride, bismuth nitrate and bismuth oxide.

[0012] It is further defined that the organic dispersant in (1) is a mixture of one or more of citric acid, sodium citrate, polyvinyl pyrrolidone, octadecylamine, hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate and dodecyl mercaptan.

[0013] It is further limited that the solvent in (1) is a mixture of one or more of ethanol, acetone, ethylene glycol, ethyl acetate, dichloromethane, methyl chloride, dimethylformamide, ethylene glycol ether, 1,2-ethylene glycol, and ethylene glycol butyl ether, or a mixture of water and one or more of ethanol, acetone, ethylene glycol, ethyl acetate, dichloromethane, methyl chloride, dimethylformamide, ethylene glycol ether, 1,2-ethylene glycol, and ethylene glycol butyl ether.

[0014] It is further defined that the total concentration of the silver metal salt and the bismuth metal salt in the precursor solution of (1) is 0.01 to 10 mol / L.

[0015] It is further defined that the molar content of the bismuth salt in the precursor solution is 0.0001 to 30% of the total molar content of the metal salt.

[0016] It is further defined that the concentration of the organic dispersant in the precursor solution of (1) is 0.1 to 10 g / L.

[0017] It is further defined that the reducing agent in (2) is a mixture of one or more of hydrazine hydrate, sodium borohydride, potassium borohydride, sodium hypophosphite, polyol, and ascorbic acid.

[0018] It is further defined that the reducing agent concentration in the reducing agent solution of (2) is 0.1 to 10 mol / L.

[0019] It is further defined that the total molar ratio of the reducing agent added in (2) to the metal salt in the precursor solution is (1-5):1.

[0020] It is further defined that (2) under medium to low temperature conditions, the reaction temperature is -50 to 50°C, the reaction time is 2 to 60 minutes, and the stirring speed is 200 to 2000 r / min.

[0021] It is further defined that the mixing method of the precursor solution and the reducing agent solution in (2) includes dropping the reducing solution into the precursor solution, or directly pouring the reducing solution into the precursor solution.

[0022] It is further defined that the reducing solution is added dropwise into the precursor solution at a rate of 0.01 to 5 mL / s.

[0023] The second object of the present invention is to provide a supersaturated silver-bismuth solid solution nanoparticle prepared by the above method, wherein the molar content of bismuth element in the nanoparticle is 0.0001-30%, and the particle size is 5-500nm.

[0024] The third object of the present invention is to provide a sintering slurry, which is specifically composed of supersaturated silver-bismuth solid solution nanoparticles prepared by the above method, organic solution, dispersant, flux and binder in a mass percentage of 50-90%: 5-45%: 0.01-5%: 0.01-5%: 0.01-5%, and the solid content of the sintering slurry is more than 80%.

[0025] It is further defined that the organic solution is a mixture of one or more of ethanol, ethylene glycol, diethylene glycol, triethylene glycol, terpineol, polyethylene glycol, glycerol, and ethyl acetate.

[0026] It is further defined that the dispersant is a mixture of one or more of citric acid, sodium citrate, β-cyclodextrin, octadecylamine, hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, and dodecylmercaptan.

[0027] It is further defined that the soldering flux is rosin resin or a rosin resin derivative; and the binder is a mixture of one or more of stearic acid, fish oil, polyethylene terephthalate, and epoxy resin.

[0028] The fourth object of the present invention is to provide a low-temperature sintering method for the above-mentioned sintering slurry, which method is: screen printing the sintering slurry on the substrate pad, aligning and placing the chip, hot pressing and sintering at a temperature above 180°C, a sintering pressure of 0 to 30 MPa, and sintering for 5 to 200 minutes.

[0029] Beneficial effects:

[0030] The present invention adopts a low-temperature in-situ chemical synthesis method, and the solubility and concentration of silver metal salt and bismuth metal salt are simultaneously improved by selecting a suitable solvent, and a liquid phase rapid non-steady-state reaction is realized by means of a strong reducing agent, and the two metal ions of silver and bismuth are rapidly reduced in-situ synchronously, so that the metal rapidly nucleates and grows in the liquid phase, and under the influence of the non-steady-state reaction mechanism, the bismuth atoms are neatly arranged in the silver metal face-centered cubic lattice, forming a non-steady-state but stable silver lattice silver-bismuth binary single-phase supersaturated solid solution, wherein the bismuth content far exceeds the bismuth content in the thermodynamically stable silver-bismuth solid solution alloy, and is stably present in nanoparticles, forming a single-phase solid solution with an average particle size of 5nm to 500nm. Although the solid solution is in a supersaturated state at room temperature in a macroscopic state, it can be stably present for a long time at a nanometer size.

[0031] The above solid solution is further prepared into a nano-paste, which relies on a high content of silver components to ensure the thermal conductivity and electrical conductivity of the solder joint. The doped low-melting-point metal bismuth can reduce the sintering temperature of the paste, sintering at ultra-low temperatures of 180°C or even lower, and has low requirements for the sintering process. It can be sintered in the air, and effectively alleviates the electromigration effect of the solder joint and reduces the cost of the paste. Through the specified sintering process, high thermal conductivity, high strength, and high reliability packaging solder joints are finally obtained. Experimental results show that the shear strength of the sintered solder joint is 12-40MPa, and the thermal conductivity is 100-300W / (m·K).

[0032] In addition, after sintering, bismuth elements precipitate at the grain boundaries of the nano-slurry to achieve the purpose of grain boundary strengthening. Combined with the introduction of bismuth elements, the electromigration and electrochemical migration effects of silver elements are effectively prevented, greatly improving the reliability of power devices.

[0033] In summary, the above-mentioned nano-slurry provided by the present invention can meet the needs of power devices with poor heat resistance and low temperature sintering, and meet their high thermal conductivity requirements. It can be used for gradient interconnected 3D multi-dimensional packaging device interconnections. The low sintering temperature saves energy and process costs. The residual thermal stress inside the solder joint is low, and it can be adapted to thinner solder joint processes. It does not require high-thickness solder joints to relieve thermal stress, further reducing process costs. In addition, it can also match the existing tin-based production line process window. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 TEM images of supersaturated nano-silver-bismuth alloy nanoparticles prepared in Example 1 (different magnifications);

[0035] Figure 2 The XRD pattern of the supersaturated silver-bismuth alloy nanoparticles prepared in Example 1;

[0036] Figure 3 This is an optical photograph of the interface of the nano-slurry prepared in Example 1 after sintering at 180°C;

[0037] Figure 4 This is an optical photograph of the interface of the nano-slurry prepared in Example 1 after sintering at 190°C;

[0038] Figure 5 This is a SEM image of the alloy nanoparticles prepared in Comparative Example 1;

[0039] Figure 6 This is the XRD pattern of the alloy nanoparticles prepared in Comparative Example 1. DETAILED DESCRIPTION

[0040] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0041] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0042] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0043] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art, and the purity of the solid and liquid reagents used is analytically pure.

[0044] Example 1

[0045] (1) The method for preparing supersaturated nano silver-bismuth alloy nanoparticles in this embodiment is carried out according to the following steps:

[0046] Step 1: Add silver metal salt AgNO3 and bismuth metal salt Bi(NO3)3 as precursors into a reaction vessel at a molar ratio of 20:1, and then add β-cyclodextrin as an organic dispersant, wherein the molar ratio of the total molar amount of metal salt in the precursor to the molar amount of the organic dispersant is 5:1, and then add a mixed solution of ethylene glycol and diethylene glycol, the total molar concentration of the metal salt is 0.2 mol / L, and the volume ratio of ethylene glycol and diethylene glycol is 1:1. Stir thoroughly at a stirring speed of 200 r / min and a stirring time of 20 min.

[0047] Step 2: After the precursor solution is evenly mixed, 20 mL of 99% pure hydrazine hydrate is used as a reducing agent, which is placed in a syringe and quickly injected into the precursor solution in a short time, while stirring at a speed of 400 r / min;

[0048] Step 3: After the reaction is completed, the obtained reactant is centrifuged at a speed of 4000 r / min for 15 minutes, the upper solution is removed and the precipitate is obtained, and then it is washed alternately with acetone, deionized water and ethanol for three times to obtain single-phase supersaturated silver-bismuth alloy nanoparticles.

[0049] The supersaturated silver-bismuth alloy nanoparticles obtained above were characterized, and the TEM characterization results are as follows: Figure 1 As shown by Figure 1 It can be seen that the obtained particles are nano-sized particles, and the bismuth element is evenly mixed in the silver metal lattice to form super-saturated silver-bismuth alloy nanoparticles. The XRD characterization results are as follows: Figure 2 ,Depend on Figure 2 It can be seen that the obtained particles only have silver metal lattice peaks, but no bismuth metal lattice peaks, indicating that a single-phase supersaturated silver-bismuth alloy has been prepared.

[0050] (2) The method for preparing a sintering slurry using the supersaturated nano silver-bismuth alloy nanoparticles prepared above is carried out according to the following steps:

[0051] Step 1: 0.7 g of supersaturated silver-bismuth alloy nanoparticles, 0.1 g of polyethylene glycol, 0.5 g of ethanol, 0.5 g of pine alcohol, 0.1 g of stearic acid and 0.1 g of rosin resin are mixed to obtain a solid-liquid mixture.

[0052] Step 2: Use a slurry mixer to fully mix the above mixture, let it stand to evaporate the ethanol, and prepare a sintering slurry.

[0053] The sintering slurry obtained above was screen-printed on the pad of the substrate and sintered at 180°C and 5 MPa for 60 min to obtain a sintering interface such as Figure 3 As shown by Figure 3 It can be seen that the nano-paste and the copper pad interface are well interconnected, forming a tight metallurgical connection, and the internal porosity of the sintered body is low, indicating that the solder joint performance is good.

[0054] The sintering slurry obtained above was screen-printed on the substrate pad and sintered at 190°C and 5 MPa for 60 min to obtain a sintering interface such as Figure 4 As shown by Figure 4 It can be seen that the nano-paste and the copper pad interface are well interconnected, forming a close metallurgical connection, and the internal porosity of the sintered body is further reduced, indicating that the solder joint performance is better than that at 180 °C.

[0055] Example 2

[0056] The difference between this embodiment and embodiment 1 is that the molar ratio of silver metal salt AgNO3 and bismuth metal salt Bi(NO3)3 is 3:1, and the remaining process steps and parameter settings are the same as those in embodiment 1.

[0057] Comparative Example 1

[0058] The difference between this comparative example and Example 1 is that the solvent is deionized water, and the other process steps and parameter settings are the same as those in Example 1.

[0059] The microstructure of the alloy nanoparticles obtained in this comparative example was characterized. Figure 5 As shown by Figure 5 It can be seen that the obtained alloy nanoparticles are nanoscale particles. Further combined with its XRD spectrum, that is, Figure 6It can be seen that the alloy nanoparticles contain Bi and bismuth oxide components in addition to the silver component. This is because the bismuth salt that provides the bismuth element is difficult to dissolve in large quantities in water. In addition, the chemical potentials of silver ions and bismuth ions in the solution are quite different. Therefore, the difference in reaction speed makes it difficult for the two metals to react simultaneously. Nano silver particles and bismuth particles are synthesized and precipitated in the solution in two steps. Due to the active nature of the bismuth element, nano bismuth particles are easily oxidized during the preparation process and in the air to form a bismuth oxide structure. Therefore, it is impossible to stably synthesize nanoparticles in a supersaturated state. This type of nanoparticle does not have sintering properties, and it is difficult to obtain a stable metallurgical connection even at 250°C.

[0060] Although the present invention has been disclosed as above in the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A method for preparing supersaturated silver-bismuth solid solution nanoparticles, characterized in that: include: (1) placing a silver metal salt and a bismuth metal salt in a reaction container in proportion, adding an organic dispersant and a solvent, and stirring until completely dissolved to obtain a precursor solution; (2) The precursor solution and the reducing agent solution are mixed and reacted under low temperature conditions to obtain silver-bismuth solid solution nanoparticles.

2. The preparation method according to claim 1, characterized in that: (1) The silver metal salt is a mixture of one or more of silver nitrate, silver sulfate, silver oxalate, silver chloride, silver bromide and silver iodide; the bismuth metal salt is a mixture of one or more of bismuth nitrate, bismuth chloride, bismuth nitrate and bismuth oxide; the organic dispersant is a mixture of one or more of citric acid, sodium citrate, polyvinyl pyrrolidone, octadecylamine, hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate and dodecyl mercaptan; the solvent is a mixture of one or more of ethanol, acetone, ethylene glycol, ethyl acetate, dichloromethane, methyl chloride, dimethylformamide, ethylene glycol ether, 1,2-ethylene glycol and ethylene glycol butyl ether, or a mixture of water and one or more of ethanol, acetone, ethylene glycol, ethyl acetate, dichloromethane, methyl chloride, dimethylformamide, ethylene glycol ether, 1,2-ethylene glycol and ethylene glycol butyl ether.

3. The preparation method according to claim 1, characterized in that: (1) The total concentration of silver metal salt and bismuth metal salt in the precursor solution is 0.01-10 mol / L; the concentration of the organic dispersant is 0.1-10 g / L.

4. The preparation method according to claim 1, characterized in that: (2) The reducing agent is a mixture of one or more of hydrazine hydrate, sodium borohydride, potassium borohydride, sodium hypophosphite, polyol, and ascorbic acid.

5. The preparation method according to claim 1, characterized in that: The reducing agent concentration in the reducing agent solution of (2) is 0.1-10 mol / L, and the total molar ratio of the added reducing agent to the metal salt in the precursor solution is (1-5):

1.

6. The preparation method according to claim 1, characterized in that: (2) Under medium and low temperature conditions, the reaction temperature is -50 to 50°C, the reaction time is 2 to 60 minutes, and the stirring speed is 200 to 2000 r / min.

7. A supersaturated silver-bismuth solid solution nanoparticle prepared by the method according to any one of claims 1 to 6, characterized in that: The molar content of bismuth element in the nanoparticles is 0.0001-30%, and the particle diameter is 5-500nm.

8. A sintering slurry, characterized in that: The supersaturated silver-bismuth solid solution nanoparticles according to claim 7, an organic solution, a dispersant, a flux and a binder are composed in a mass percentage of 50-90%: 5-45%: 0.01-5%: 0.01-5%: 0.01-5%, and the solid content of the sintering slurry is more than 80%.

9. The sintering slurry according to claim 8, characterized in that: The organic solvent is a mixture of one or more of ethanol, ethylene glycol, diethylene glycol, triethylene glycol, terpineol, polyethylene glycol, glycerol, and ethyl acetate; the dispersant is a mixture of one or more of citric acid, sodium citrate, β-cyclodextrin, octadecylamine, hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, and dodecyl mercaptan; the soldering flux is rosin resin or a rosin resin derivative; the binder is a mixture of one or more of stearic acid, fish oil, polyethylene terephthalate, and epoxy resin.

10. A low temperature sintering method for the sintering slurry according to claim 8 or 9, characterized in that: The sintering slurry is screen-printed on the pad of the substrate, the chip is aligned and placed, and hot-pressed sintering is performed at a temperature above 180° C. and a sintering pressure of 0 to 30 MPa for 5 to 200 minutes.

Citation Information

Patent Citations

  • Nano intermetallic compound soldering paste and preparation method thereof

    CN102922177A

  • Method for making modified sliver powder and non-glass powder sintered type elargol

    CN104240842A

  • Alloy silver powder, preparation method thereof and solar conductive slurry prepared therefrom

    CN106229026A

  • Production method of superfine silver and bismuth alloy powder for solar cell silver paste

    CN110385442A

  • Nano silver-copper solid solution, and preparation method and application thereof

    CN113593772A