Machining method for complex thin-wall cast aluminum alloy part
Through low-pressure digital-module casting, solid solution treatment, sandblasting and multi-stage aging treatment, combined with five-axis processing and grinding processes, the deformation and clamping problems of complex thin-wall casting parts during processing are solved, achieving high precision and high efficiency Processing effect.
Patent Information
- Application Number
- CN202410958232.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
AI Technical Summary
Complex thin-wall cast aluminum alloy parts are prone to deformation during processing, making it difficult to achieve precise clamping and high-quality processing, especially in complex cavity structures such as deep cavity and narrow grooves. Traditional methods are difficult to provide sufficient support, resulting in tremor. Vibration, cutting tool and processing stress deformation problems.
Using low-pressure digital-module casting, solid solution treatment, sandblasting treatment, multi-stage aging treatment and five-axis machining center combined with grinding technology, special clamping tools and bonding technology are designed to ensure processing stability by gradually releasing stress and improving parts rigidity. and precision.
It significantly improves the dimensional stability and surface finish of the parts, reduces clamping difficulty, improves processing quality and efficiency, and ensures high-precision processing in thin-walled areas and the mechanical performance of the parts.
Smart Images

Figure CN118875652A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of parts processing, in particular to a method for processing complex thin-wall cast aluminum alloy parts. Background Art
[0002] Complex thin-walled casting parts are widely used in aerospace, automobile manufacturing, precision instruments and other fields. These parts have extremely high requirements for processing technology due to their unique structural design and material properties. The thin-walled characteristics make it very easy to deform during processing, especially in the processing stages such as milling and drilling that remove a large amount of material; during casting and subsequent mechanical processing, thin-walled structures are easily deformed by thermal stress and mechanical stress, affecting the dimensional stability and assembly performance of the final parts. Although the thin-wall design reduces weight, it also reduces the strength and rigidity of the parts. Vibration is prone to occur during processing, affecting the processing quality. When processing thin-walled areas, how to avoid chatter and tool breakage caused by the tool, and how to effectively support the parts to avoid processing stress deformation are the main technical challenges.
[0003] Traditional processing methods often fail to provide sufficient support force, especially when processing complex cavities such as deep cavities and narrow grooves. The cutting force of the tool will cause the workpiece to vibrate, affecting the processing accuracy and surface finish. In addition, due to the fragility of thin-walled structures, improper clamping methods can also cause the workpiece to break.
[0004] To this end, those skilled in the art have proposed a method for processing complex thin-walled cast aluminum alloy parts to solve the problems raised in the background art. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for processing complex thin-walled cast aluminum alloy parts to solve the problems of the prior art in processing complex thin-walled cast aluminum alloy parts, such as difficulty in clamping and locating the thin wall due to the cavity structure, and insufficient rigidity.
[0006] A method for processing a complex thin-walled cast aluminum alloy part comprises the following steps:
[0007] S1. Use low-pressure digital model casting - ZL114A material; according to the three-dimensional casting model, leave 4-6mm on one side of the contour; because the internal cavity of the structural frame cannot be effectively processed, low-pressure digital model casting is used, and the area with appearance and precision requirements is left with margins to prepare for future processing;
[0008] S2, solution treatment, heating to 530-540℃, keeping warm for 4-6 hours, cooling in air to release the stress generated by casting;
[0009] S3, sandblasting to remove the residual material in the inner cavity and eliminate some internal stress;
[0010] S4. The fitter draws the lines with uniform allowance. The fitter uses the unprocessed surface of the inner cavity as a reference and evenly divides the allowance to draw the contour line of the outer shape to prepare for rough processing;
[0011] S5. Refer to the markings, rough mill the six sides of the outer shape and the inner cavity, and leave a single-side machining allowance of 2mm to prepare for the subsequent semi-finishing milling;
[0012] S6. Perform high temperature aging treatment;
[0013] S7, semi-finishing milling of the six outer surfaces and inner cavity;
[0014] S8, performing medium temperature aging treatment and standing for more than 96 hours to further release stress;
[0015] S9, semi-finishing milling of the six outer surfaces and the inner cavity;
[0016] S10, perform low temperature aging treatment to further stabilize the size;
[0017] S11, grinding process reference surface to a flatness of 0.01mm, obtaining the processing process reference;
[0018] S12. Using the grinding process reference surface as a reference, the five-axis machining center worktable processes the relative position holes to obtain the required accuracy of each hole drawing.
[0019] Preferably, a plurality of positioning grooves are provided on the surface of the worktable of the five-axis machining center in the S, a plurality of external pressure plates and internal pressure plates are installed on the inner wall of the positioning groove, an external pressure plate bolt is installed on the inner wall of the external pressure plate, and an internal pressure plate bolt is installed on the inner wall of the internal pressure plate.
[0020] Preferably, an external pressure plate gasket is provided on the bottom surface of the external pressure plate, an internal pressure plate gasket is provided between the internal pressure plate and the internal pressure plate bolt, and a plurality of adhesive blocks are provided on the side wall of the internal pressure plate.
[0021] Preferably, the heating temperature in S6 reaches 160-180° C., and after keeping the temperature for 3-5 hours, it is naturally air-cooled to release the processing stress generated by the rough processing.
[0022] Preferably, during the semi-finishing milling in S7, a single-sided semi-finishing allowance of 1 mm is left to prepare for final finishing.
[0023] Preferably, the heating temperature in S8 reaches 120-140° C., followed by natural air cooling to release the processing stress generated by rough processing.
[0024] Preferably, in the S9, 0.3 mm is left on one side in the precision area, the non-precision area is processed and formed, and the process reference surface is precision milled to ensure a flatness of 0.03 mm.
[0025] Preferably, the low temperature aging treatment in S10 is to cool the workpiece at a temperature below -70°C.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The method adopts rough milling, semi-finishing milling and finishing milling first, and intersperses solid solution treatment, sandblasting and aging treatment (3 times) for stabilization. Specifically, stress relief annealing (solid solution treatment) is performed after casting, sandblasting is performed to remove surface blank residue and stress relief, aging treatment, rough machining, aging treatment, semi-finishing, aging treatment and finishing. In finishing, the fitter cooperates with the grinding process reference surface, and then designs a special clamping tool combined with bonding, so that the part is in a natural clamping state during the milling process, the chip force is transmitted in parallel, and the stability is greatly increased. The method cleverly solves the problem of large clamping deformation of special-shaped and complex thin-walled cast aluminum parts. For small and medium-sized batches, difficult to clamp and align, structurally special-shaped, and large-deformation thin-walled casting parts, unique processing clamping methods and heat treatment processes are used, and the auxiliary tooling is simple, which reduces the difficulty of clamping and improves the processing quality and efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a schematic diagram of the structure of the five-axis machining center worktable clamping the parts to be processed;
[0029] Figure 2 It is a structural diagram of the workbench of the five-axis machining center;
[0030] Figure 3 It is a heat treatment process flow chart of the present invention;
[0031] Figure 4 This is the process flow chart of this part processing method.
[0032] In the figure:
[0033] 1. Worktable of five-axis machining center; 101. Positioning groove; 2. External pressure plate; 3. External pressure plate gasket; 4. External pressure plate bolt; 5. Adhesive block; 6. Internal pressure plate; 7. Internal pressure plate bolt; 8. Internal pressure plate gasket; 9. Parts to be processed. DETAILED DESCRIPTION
[0034] The following is a further detailed description of the embodiments of the present invention in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.
[0035] Embodiment 1: As shown in the attached Figure 1 To Attachment Figure 4 As shown: The present invention provides a method for processing a complex thin-walled cast aluminum alloy part, comprising the following steps:
[0036] S1. Use low-pressure digital model casting - ZL114A material; according to the three-dimensional casting model, leave 4-6mm on one side of the contour; because the internal cavity of the structural frame cannot be effectively processed, low-pressure digital model casting is used, and the area with appearance and precision requirements is left with margins to prepare for future processing;
[0037] S2, solution treatment, heating to 530-540℃, keeping warm for 4-6 hours, cooling in air to release the stress generated by casting;
[0038] S3, sandblasting to remove the residual material in the inner cavity and eliminate some internal stress;
[0039] S4. The fitter draws the lines with uniform allowance. The fitter uses the unprocessed surface of the inner cavity as a reference and evenly divides the allowance to draw the contour line of the outer shape to prepare for rough processing;
[0040] S5. Refer to the markings, rough mill the six sides of the outer shape and the inner cavity, and leave a single-side machining allowance of 2mm to prepare for the subsequent semi-finishing milling;
[0041] S6. Perform high temperature aging treatment, heating the temperature to 160-180°C, keep warm for 3-5 hours, and then naturally air cool to release the processing stress caused by rough processing;
[0042] S7, semi-finishing milling of the six outer surfaces and the inner cavity, leaving a semi-finishing allowance of 1mm on one side to prepare for the final finishing;
[0043] S8, perform medium temperature aging treatment, heating the temperature to 120-140°C, then naturally air cool, and stand for more than 96 hours to release the processing stress caused by rough processing;
[0044] S9, semi-finish milling the six sides of the outer shape and the inner cavity again, leaving 0.3mm on one side of the precision area, processing and forming the non-precision area, and precision milling the process reference surface at the same time to ensure the flatness of 0.03mm;
[0045] S10, perform low temperature aging treatment, cool the workpiece below -70°C to further stabilize the size;
[0046] S11, grinding process reference surface to a flatness of 0.01mm, obtaining the processing process reference;
[0047] S12. Using the grinding process reference surface as a reference, the five-axis machining center worktable 1 processes the relative position holes to obtain the required accuracy of each hole drawing.
[0048] As can be seen from the above, low-pressure digital die casting---ZL114A material is used. The maximum size of the part is 927×712×67.5. The D surface is mainly used as the reference surface. The thin walls in many places in the structure cavity are only 3mm thick, and the eight places are coplanar within 0.01. The flatness requirement is 0.01, which is the second-level processing accuracy. The main accuracy requirements are the verticality and position of the hole tolerances of Φ2, Φ3, Φ4, Φ5 and Φ6 to the D reference surface of 0.02, and the parallelism of the grooves, bosses and the reference surface requires 0.02. The overall processing plan: rough milling, semi-finishing milling, and finishing milling (fitter cooperates with the grinding process reference surface), the verticality and position of the hole tolerances of Φ2, Φ3, Φ4, Φ5 and Φ6 to the D reference surface, and the parallelism of the grooves, bosses and the reference surface are required to be processed by a five-axis machining center, and the solid solution treatment is interspersed in the middle. The processing includes the following steps: rough machining, sandblasting, aging treatment (3 times) and stabilization treatment, specifically, stress relief annealing (solid solution treatment) after casting, sandblasting to remove surface roughcast residue and stress relief, aging treatment (165°C), rough machining, aging treatment, semi-finishing, aging treatment, and finishing; in finishing, the fitter cooperates with the grinding process reference surface, and then designs special clamping tools combined with special bonding technology to make the part in a natural clamping state during the milling process, and the cutting force is transmitted in parallel, which greatly increases the stability and cleverly solves the problem of large clamping deformation of special-shaped and complex thin-walled cast aluminum parts; this method is suitable for small and medium-sized batches, difficult to clamp and align, structurally special-shaped, and large-deformation thin-walled casting parts, with unique processing clamping methods and heat treatment processes, simple auxiliary tooling (establishing process reference surfaces), reducing the difficulty of clamping, and improving processing quality and efficiency.
[0049] By adopting low-pressure digital model casting technology (ZL114A material), combined with precise solid solution, aging treatment and multi-stage machining, the stress during casting and machining is effectively controlled, and the dimensional stability and surface finish of the parts are significantly improved, especially in the thin-wall area, ensuring high precision requirements;
[0050] The phased aging treatment (high temperature, medium temperature and low temperature) strategy ensures that the internal stress generated at different processing stages is effectively released. In particular, the low temperature aging treatment further stabilizes the part size and reduces the risk of deformation during subsequent processing and use.
[0051] Through the step-by-step implementation of bench marking, semi-finishing and finishing, a reasonable processing allowance is reserved for each step, ensuring that while gradually approaching the final size, the processing error can also be adjusted and corrected in time, improving the controllability and efficiency of the entire processing process;
[0052] By grinding the reference surface to an extremely high degree of flatness and using it as a reference for subsequent five-axis machining, it is ensured that the machining accuracy of each hole position meets the requirements of the drawing, thereby improving the interchangeability and consistency of the overall assembly.
[0053] This processing method not only focuses on the accuracy of size and shape, but also effectively improves the mechanical properties of aluminum alloy parts through the optimization of material processing and processing technology, improves the strength and toughness of parts, and enables the final parts to maintain good performance under complex working conditions.
[0054] Embodiment 2: As shown in the attached Figure 1 To Attachment Figure 2 As shown: This embodiment is basically the same as the previous embodiment, except that, in S12, a plurality of positioning grooves 101 are opened on the surface of the worktable 1 of the five-axis machining center, and a plurality of external pressure plates 2 and internal pressure plates 6 are installed on the inner wall of the positioning groove 101. The inner wall of the external pressure plate 2 is installed with an external pressure plate bolt 4, and the inner wall of the internal pressure plate 6 is installed with an internal pressure plate bolt 7. First, place the part 9 to be processed on the worktable 1 of the five-axis machining center, and the grinding process reference surface is in full contact with the worktable. The external pressure plate 2, the external gasket 3, and the external pressure plate bolt 4 jointly fix the side square hole and the top of the part to be processed. The inner cavity is fixed by a special internal pressure plate 6, an internal pressure plate bolt, and an internal gasket 8 to prevent the parts from being deformed by pressure. Adhesive blocks 5 are added at the connection gap to effectively reduce the deformation of thin-walled parts and ensure the accuracy of processed parts.
[0055] An external pressing plate gasket 3 is provided on the bottom surface of the external pressing plate 2 , an internal pressing plate gasket 8 is provided between the internal pressing plate 6 and the internal pressing plate bolt 7 , and a plurality of adhesive blocks 5 are provided on the side wall of the internal pressing plate 6 .
[0056] As can be seen from the above, when clamping parts, first place the parts flat on the workbench 1 of the five-axis machining center in a natural state, while ensuring that the grinding reference surface is in contact with the workbench. The auxiliary support surface is pressed tightly with the external pressure plate bolts 4 and the external pressure plate 2 at the square grooves on the left and right sides. The inner side of the part is fixed by the internal pressure plate 6 combined with the adhesive block 5. In order to prevent deformation of the parts during clamping and insufficient structural rigidity, multiple auxiliary fixations are used to meet the requirements of cutting and clamping, and the following order is strictly followed:
[0057] 1. Place the workpiece flat on the work surface in its natural state, and grind the reference surface to contact the work surface. Use a level to check whether it is flat and the contact surface is qualified. The table runout is within 0.01.
[0058] 2. Clamp the square groove pressure plates on both sides, press the gauge when tightening, and observe the fluctuation of the gauge needle;
[0059] 3. Use alcohol to clean multiple fixed contact surfaces of parts (to remove oil and increase contact force). Use AB glue to fix and bond the auxiliary tooling to the side of the parts. The AB glue is milky white when it is dry. Blowing can speed up the drying of the glue. Use a thin tool to remove the glue and gently lift the workpiece.
[0060] 4. After processing, remove the glue from the workpiece and gently wipe it with alcohol cotton yarn (if there is glue residue on the surface of the workpiece, spray the appropriate glue remover again. Pay attention to safety during the process, as glue removal may cause slight corrosion to the skin);
[0061] For this type of auxiliary thin-wall casting cavity workpiece processing, special fixtures combined with AB glue bonding keep the workpiece in a natural state with minimal deformation and maximum dimensional stability.
[0062] The five-axis machining center worktable 1 utilizes a combination of an external pressure plate, an internal pressure plate and an adhesive block to achieve stable and precise clamping of parts. This method not only avoids the deformation problem that may be caused by traditional clamping methods, but also makes full use of the natural state of the workpiece, maximizes its structural rigidity, and thus improves the precision control during the machining process.
[0063] The embodiments of the present invention are provided for the purpose of illustration and description. Although the embodiments of the present invention have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations of the present invention. Ordinary technicians in this field can change, modify, replace and deform the above embodiments within the scope of the present invention.
[0064] In the description of the present invention, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. "Multiple" means two or more, unless otherwise clearly and specifically defined.
[0065] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0066] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0067] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory.
[0068] In the drawings of the embodiments disclosed in the present invention, only the structures involved in the embodiments disclosed in the present invention are involved, and other structures can refer to the general design. In the absence of conflict, the same embodiment and different embodiments of the present invention can be combined with each other.
[0069] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for processing complex thin-walled cast aluminum alloy parts, characterized in that: The following steps are involved: S1. Use low-pressure digital mold casting - ZL114A material; according to the three-dimensional casting model, leave 4-6mm on one side of the contour; S2, solution treatment, heating to 530-540℃, keeping warm for 4-6 hours, cooling in air; S3, sandblasting to remove residual material residue in the inner cavity; S4, fitter marking, the allowance is uniform; S5. Refer to the marking line, rough mill the six sides of the outer shape and the inner cavity, leaving a single-side machining allowance of 2mm; S6. Perform high temperature aging treatment; S7, semi-finishing milling of the six outer surfaces and inner cavity; S8, performing medium temperature aging treatment and standing for more than 96 hours to further release stress; S9, semi-finishing milling of the six outer surfaces and the inner cavity; S10, perform low temperature aging treatment to further stabilize the size; S11, grinding process reference surface to a flatness of 0.01mm, obtaining the processing process reference; S12. Using the grinding process reference surface as a reference, the five-axis machining center worktable (1) processes the holes in relative positions to obtain the accuracy required by the drawing for each hole.
2. A method for processing complex thin-walled cast aluminum alloy parts as claimed in claim 1, characterized in that: A plurality of positioning grooves (101) are provided on the surface of the worktable (1) of the five-axis machining center in S12, and a plurality of external pressure plates (2) and internal pressure plates (6) are installed on the inner walls of the positioning grooves (101), and external pressure plate bolts (4) are installed on the inner walls of the external pressure plates (2), and internal pressure plate bolts (7) are installed on the inner walls of the internal pressure plates (6).
3. A method for processing a complex thin-walled cast aluminum alloy part as claimed in claim 2, characterized in that: An external pressure plate gasket (3) is provided on the bottom surface of the external pressure plate (2), an internal pressure plate gasket (8) is provided between the internal pressure plate (6) and the internal pressure plate bolt (7), and a plurality of adhesive blocks (5) are provided on the side wall of the internal pressure plate (6).
4. A method for processing a complex thin-walled cast aluminum alloy part as claimed in claim 3, characterized in that: In S6, the heating temperature reaches 160-180° C., and after being kept warm for 3-5 hours, it is naturally air-cooled to release the processing stress caused by the rough processing.
5. A method for processing a complex thin-walled cast aluminum alloy part as claimed in claim 4, characterized in that: During the semi-finishing milling in S7, a single-sided semi-finishing allowance of 1 mm is left.
6. A method for processing a complex thin-walled cast aluminum alloy part as claimed in claim 1, characterized in that: In S8, the heating temperature reaches 120-140° C., followed by natural air cooling.
7. A method for processing complex thin-walled cast aluminum alloy parts as claimed in claim 1, characterized in that: The S9 medium-precision area has a single side retention of 0.3mm, and the non-precision area is processed and formed, and the process reference surface is precision milled to ensure a flatness of 0.03mm.
8. A method for processing a complex thin-walled cast aluminum alloy part as claimed in claim 1, characterized in that: The low temperature aging treatment in S10 is to cool the workpiece below -70°C.
Citation Information
Cited By
Three-in-one motor and processing method of motor shell of three-in-one motor
CN120244479A
7075 aluminum alloy polyhedral part machining process
CN121042831A