Preparation process of environment-friendly cold-resistant polyvinyl chloride elastomer material for elevator

By adjusting the ratio of polyvinyl chloride resin additives and nanomaterials, combining vacuum technology and environmentally friendly rare earth heat stabilizers, the performance and environmental protection problems of polyvinyl chloride elastomer materials in elevator applications are solved, and high cold resistance and Preparation of high-density polyvinyl chloride elastomer materials.

CN118876260AInactive Publication Date: 2024-11-01NANTONG XING HUA DA GAO IND CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410556710.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-07
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In elevator applications, existing polyvinyl chloride elastomer materials have problems such as poor mechanical properties and cold resistance, insufficient material compactness, high content of harmful substances in waste gas during production, and poor performance and stability.

Method used

Adopt an environmentally friendly cold-resistant polyvinyl chloride elastomer material preparation process for elevators, including raw material preparation, premix, melt blending, crosslinking reaction, vacuum exhaust and plasticizing molding steps, by adjusting polyvinyl chloride resin additives and nanometers The proportion of materials is to use vacuum technology to remove bubbles, and choose environmentally friendly rare earth heat stabilizers and phenolic resin crosslinkers to optimize process conditions to improve the cold resistance, compactness and environmental protection of the materials.

Benefits of technology

It significantly improves the cold resistance, mechanical properties and environmental protection of polyvinyl chloride elastomer materials, reduces bubble and crack defects, enhances the mechanical properties and thermal stability of the materials, meets the application needs of elevator compensation chains, and reduces energy. Consumption and waste generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118876260A_ABST
    Figure CN118876260A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation process of an environment-friendly cold-resistant polyvinyl chloride elastomer material for an elevator, and relates to the technical field of material preparation. S1, raw material preparation; s2, performing premixing; s3, carrying out melt blending; s4, carrying out a cross-linking reaction; s5, performing vacuum exhaust; s6, plastifying and forming; and S7, carrying out post-treatment. The cold resistance of the polyvinyl chloride material can be improved by adjusting the polyvinyl chloride resin auxiliary agent, the freezing point of various plasticizers is effectively reduced by the ethyl acid ester, the effect of enhancing the cold resistance of the film is achieved, the cold resistance of the polyvinyl chloride product can be improved by adding the polyacrylate elastomer into the polyvinyl chloride resin, and the cold resistance of the film is improved. In the preparation process of the polyvinyl chloride elastomer material, the glass transition temperature of the polyvinyl chloride resin is reduced by the chlorinated paraffin plasticizing regulator, so that the cold resistance of the polyvinyl chloride resin is improved, the matrix can be refined by the nano silicon dioxide, the compactness and the impact resistance of the material are improved, and the application requirement of the polyvinyl chloride elastomer material in the elevator compensation chain is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material preparation, and in particular to a preparation process of an environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators. Background Art

[0002] Polyvinyl chloride elastomer material is a new type of elastomer material that is mainly made of PVC, which is blended with elastomers, introduced with cross-linked or disproportionated structures, synthesized with high relative molecular weight polyvinyl chloride resins as base resins, and appropriately added with modifiers such as plasticizers. Polyvinyl chloride elastomer material has the advantages of chemical corrosion resistance, high wear resistance, good electrical insulation, and flame retardancy. It is widely used in building materials, wires and cables, medical supplies, piping systems, clothing, and footwear.

[0003] The defects of the elastomeric material preparation process in the prior art are:

[0004] 1. Patent document KR1020040065433A discloses a method for preparing a vinyl chloride thermoplastic elastomer. The mechanical properties and cold resistance of the vinyl chloride thermoplastic elastomer prepared by this method are poor, and the elastomer material is not dense enough to meet the application requirements of polyvinyl chloride elastomer materials in elevator compensation chains.

[0005] 2. Patent document CN104893152B discloses an environmentally friendly and cold-resistant polyvinyl chloride elastomer composition and a preparation method thereof. The method does not extract the air in the material when preparing the environmentally friendly and cold-resistant polyvinyl chloride elastomer composition. Bubbles exist in the prepared elastomer composition and cracks will occur. The preparation quality of the polyvinyl chloride elastomer material is poor.

[0006] 3. Patent document CN111925607B discloses a polyvinyl chloride elastomer, a preparation method and an application thereof. This method cannot reduce the content of harmful substances in the exhaust gas when preparing the polyvinyl chloride elastomer, increases energy consumption and waste generation, and cannot ensure the environmental friendliness of the polyvinyl chloride elastomer material production process.

[0007] 4. Patent document CN111019265B discloses a highly efficient antibacterial medical polyvinyl chloride elastomer. The performance and stability of the material cannot be guaranteed during the preparation of the polyvinyl chloride elastomer. The elasticity, strength and heat resistance of the polyvinyl chloride elastomer material are poor, which reduces the production quality of the polyvinyl chloride elastomer material. Summary of the invention

[0008] The purpose of the present invention is to provide a process for preparing an environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators to solve the problems raised in the above-mentioned background technology.

[0009] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a process for preparing an environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators, comprising the following steps: S1, raw material preparation; S2, premixing; S3, melt blending; S4, cross-linking reaction; S5, vacuum exhaust; S6, plasticizing and molding; S7, post-treatment.

[0010] Preferably, the raw material preparation step is as follows: by weight, prepare 100 parts of polyvinyl chloride resin, 70 to 90 parts of polyacrylate, 15 to 30 parts of nano-silica, 20 to 25 parts of chlorinated paraffin plasticizer, 10 to 15 parts of monoethyl ester, 10 to 15 parts of rare earth heat stabilizer, 1 to 5 parts of phenolic resin crosslinker, 2 to 3 parts of lubricant, 0.5 to 1 part of antioxidant and 0.5 to 0.8 part of defoamer.

[0011] Preferably, the polyvinyl chloride resin is obtained by polymerizing through a low-temperature polymerization process, followed by washing, centrifugal dehydration, and drying.

[0012] Preferably, the premixing step is as follows: premixing the polyvinyl chloride resin with polyacrylate, nano-silica, chlorinated paraffin plasticizer, monoethyl ester, rare earth heat stabilizer, lubricant, antioxidant and defoamer in a high-speed mixer to ensure that the raw materials are fully mixed evenly, the rotation speed is 3000r / min, and the mixing power is controlled at 20 to 55KW.

[0013] Preferably, the melt blending step is as follows: adding the premixed raw materials into an internal mixer for melt blending, the blending temperature is 160-180°C, the blending time is 60-90min, the rotor speed is 40-60r / min, and in the molten state, the components are fully mixed and dispersed through shearing and mixing.

[0014] Preferably, the cross-linking reaction step is as follows: adding a phenolic resin cross-linking agent to initiate a cross-linking reaction during melt blending, the blending temperature is 160-180° C., the blending time is 10-15 min, and the rotor speed is 40-60 r / min.

[0015] Preferably, the vacuum exhaust step is as follows: after the material mixing is completed, the mixed material is transferred to a vacuum kneader, the exhaust port of the vacuum kneader is closed and the vacuum pump is started to evacuate the inside of the equipment, and the vacuum degree reaches -0.09MPa and is maintained for 5 to 8 minutes to ensure that the bubbles in the material are fully extracted. After the exhaust is completed, the vacuum pump is closed and the exhaust port is opened to take out the material.

[0016] Preferably, the plasticizing and molding steps are as follows: placing the vacuum-exhausted material into a cooling agitator for cooling treatment, cooling to below 40°C, and melt-extrude the mixed material on a twin-screw extruder, wherein the front section temperature of the twin-screw extruder is 80-110°C, the middle section temperature is 130-150°C, the rear section temperature is 150-170°C, and the head temperature is 80-100°C. The extruded material is granulated to obtain a polyvinyl chloride elastomer material.

[0017] Preferably, the post-treatment steps are as follows: (1) preliminary water cooling: water cooling of the polyvinyl chloride elastomer material is achieved through one or more water cooling tanks; (2) air cooling: after water cooling, the polyvinyl chloride elastomer material is further passed through the air cooling zone of the fan to help the surface and interior of the material continue to cool down; (3) curing: the material is maintained at 80-100°C to ensure that it is fully cured.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. The present invention can improve the cold resistance of polyvinyl chloride materials by adjusting the polyvinyl chloride resin additives. The addition of nano-silicon dioxide and monoethyl ester in the preparation process of polyvinyl chloride elastomer materials can improve the cold resistance of the elastomer materials. Monoethyl ester effectively reduces the freezing point of various plasticizers to achieve the effect of strengthening the cold resistance of the film. The addition of polyacrylate elastomers to polyvinyl chloride resin can improve the cold resistance of polyvinyl chloride products. The chlorinated paraffin plasticizer regulator in the preparation process of polyvinyl chloride elastomer materials can reduce the glass transition temperature of polyvinyl chloride resin, thereby improving its cold resistance. Nano-silicon dioxide can significantly improve the mechanical properties and heat and cold resistance of polyvinyl chloride elastomer materials, refine the matrix, improve the density and impact resistance of the material, and meet the application requirements of polyvinyl chloride elastomer materials in elevator compensation chains.

[0020] 2. The present invention ensures that the material is in a vacuum state before entering the mold, and uses a vacuum pump to extract air from the material before extrusion molding to eliminate bubbles, which helps to reduce the number of bubbles in the product. During the extrusion process, the pressure and speed are controlled to ensure that the material flows evenly in the mold and reduce the generation of defects such as cracks. The chlorinated paraffin plasticizer regulator improves the processing performance of the polyvinyl chloride resin, improves the plasticizing effect of the PVC resin, reduces the generation of bubbles and cracks, ensures that the PVC resin is fully plasticized and evenly mixed, and avoids the generation of defects such as bubbles and cracks, thereby improving the quality of the polyvinyl chloride elastomer material.

[0021] 3. The present invention selects an environmentally friendly rare earth heat stabilizer in the pretreatment process, uses a high-speed mixer with good sealing and thermal efficiency in the pretreatment process to reduce exhaust gas leakage and energy consumption, avoids the use of additives containing harmful substances or difficult to degrade, and uses environmentally friendly auxiliary materials to reduce the content of harmful substances in the exhaust gas. The rare earth heat stabilizer not only has excellent thermal stabilization performance but also has coupling and toughening effects, which can promote system gelation, reduce melt viscosity and thus improve PVC processing performance. The polyvinyl chloride resin prepared by the low-temperature polymerization process further reduces energy consumption and waste generation, and improves the environmental friendliness of the polyvinyl chloride elastomer material production process.

[0022] 4. The present invention adds a phenolic resin cross-linking agent during the preparation process of the polyvinyl chloride elastomer material, adopts a chemical cross-linking method to improve the performance and stability of the material, causes a chemical reaction between the polyvinyl chloride molecular chains to form a three-dimensional network structure, thereby improving the elasticity, strength, heat resistance and other properties of the polyvinyl chloride elastomer material, ensuring that the cross-linking agent is uniformly dispersed in the polyvinyl chloride. The three-dimensional network structure can effectively improve the mechanical properties and thermal stability of the material. Chemical cross-linking can increase the elastic modulus, tensile strength, tear strength and other mechanical properties of the material, so that it has better impact resistance and deformation resistance. At the same time, chemical cross-linking can also improve the heat resistance of the material, further improving the production quality of the polyvinyl chloride elastomer material. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a process flow chart for preparing the environmentally friendly cold-resistant polyvinyl chloride elastomer material of the present invention;

[0024] Figure 2 This is a schematic diagram showing the effects of different preparation factors on the properties of elastomeric materials according to the present invention. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] In the description of the present invention, it should be noted that the terms "upper", "lower", "inner", "outer", "front end", "rear end", "two ends", "one end", "the other end" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0027] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection or a movable connection, or a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0028] Embodiment 1, an embodiment provided by the present invention: a process for preparing an environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators, comprising the following steps; S1, raw material preparation; S2, premixing; S3, melt blending; S4, plasticizing and molding; S5, post-processing.

[0029] The steps of preparing raw materials are as follows: by weight, prepare 100 parts of polyvinyl chloride resin, 15 parts of nano-activated calcium carbonate, 20 parts of phthalic acid di-plasticizer regulator, 10 parts of calcium zinc composite stabilizer, 2 parts of lubricant, 0.5 parts of antioxidant and 0.5 parts of defoamer.

[0030] The premixing steps are as follows: premix the polyvinyl chloride resin with nano-active calcium carbonate, phthalic acid displastizer, calcium-zinc composite stabilizer, lubricant, antioxidant and defoamer in a high-speed mixer to ensure that the raw materials are fully mixed evenly, the speed is 3000r / min, and the mixing power is controlled at 20KW.

[0031] The melt blending steps are as follows: add the pre-mixed raw materials into an internal mixer for melt blending, the blending temperature is 160°C, the blending time is 90min, the rotor speed is 60r / min, and in the molten state, the components are fully mixed and dispersed through shearing and mixing.

[0032] The plasticizing and molding steps are as follows: the melt-blended material is placed in a cooling agitator for cooling treatment, cooled to below 40°C, and the mixed material is melt-extruded on a twin-screw extruder, wherein the front section temperature of the twin-screw extruder is 80°C, the middle section temperature is 130°C, the rear section temperature is 150°C, and the head temperature is 80°C. The extruded material is granulated to obtain a polyvinyl chloride elastomer material.

[0033] The post-processing steps are as follows: (1) initial water cooling: water cooling of the polyvinyl chloride elastomer material is achieved through one or more water cooling tanks; (2) air cooling: after water cooling, the polyvinyl chloride elastomer material further passes through the air cooling zone of the fan to help the surface and interior of the material continue to cool down; (3) curing: the material is maintained below 80°C to ensure that it is fully cured.

[0034] Embodiment 2, an embodiment provided by the present invention: a process for preparing an environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators, comprising the following steps; S1, raw material preparation; S2, premixing; S3, melt blending; S4, plasticizing and molding; S5, post-processing.

[0035] The steps of preparing raw materials are as follows: by weight, prepare 100 parts of polyvinyl chloride resin, 15 parts of nano silicon dioxide, 20 parts of phthalic acid di-plasticizer, 10 parts of calcium zinc composite stabilizer, 2 parts of lubricant, 0.5 parts of antioxidant and 0.5 parts of defoamer.

[0036] The premixing steps are as follows: premix the polyvinyl chloride resin with nano silicon dioxide, phthalic acid dispersant, calcium zinc composite stabilizer, lubricant, antioxidant and defoamer in a high-speed mixer to ensure that the raw materials are fully mixed evenly, the speed is 3000r / min, and the mixing power is controlled at 20KW.

[0037] The melt blending steps are as follows: add the pre-mixed raw materials into an internal mixer for melt blending, the blending temperature is 160°C, the blending time is 90min, the rotor speed is 60r / min, and in the molten state, the components are fully mixed and dispersed through shearing and mixing.

[0038] The plasticizing and molding steps are as follows: the melt-blended material is placed in a cooling agitator for cooling treatment, cooled to below 40°C, and the mixed material is melt-extruded on a twin-screw extruder, wherein the front section temperature of the twin-screw extruder is 80°C, the middle section temperature is 130°C, the rear section temperature is 150°C, and the head temperature is 80°C. The extruded material is granulated to obtain a polyvinyl chloride elastomer material.

[0039] The post-processing steps are as follows: (1) initial water cooling: water cooling of the polyvinyl chloride elastomer material is achieved through one or more water cooling tanks; (2) air cooling: after water cooling, the polyvinyl chloride elastomer material further passes through the air cooling zone of the fan to help the surface and interior of the material continue to cool down; (3) curing: the material is maintained below 80°C to ensure that it is fully cured.

[0040] Depend on Figure 2 It can be seen that when the plasticizer, stabilizer and preparation conditions are consistent, the polyvinyl chloride elastomer material prepared in Example 2 using nano-silicon dioxide as the nanomaterial has a lower brittle temperature, stronger impact resistance and better cold resistance.

[0041] Embodiment 3, an embodiment provided by the present invention: a process for preparing an environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators, comprising the following steps; S1, raw material preparation; S2, premixing; S3, melt blending; S4, plasticizing and molding; S5, post-processing.

[0042] The steps of preparing raw materials are as follows: by weight, prepare 100 parts of polyvinyl chloride resin, 70 parts of polyacrylate, 15 parts of nano-silicon dioxide, 20 parts of phthalic acid di-plasticizer, 10 parts of calcium zinc composite stabilizer, 2 parts of lubricant, 0.5 parts of antioxidant and 0.5 parts of defoaming agent.

[0043] The premixing steps are as follows: premix polyvinyl chloride resin with polyacrylate, nano-silica, phthalic acid di-plasticizer, calcium zinc composite stabilizer, lubricant, antioxidant and defoamer in a high-speed mixer to ensure that the raw materials are fully mixed evenly, the speed is 3000r / min, and the mixing power is controlled at 20KW.

[0044] The melt blending steps are as follows: add the pre-mixed raw materials into an internal mixer for melt blending, the blending temperature is 160°C, the blending time is 90min, the rotor speed is 60r / min, and in the molten state, the components are fully mixed and dispersed through shearing and mixing.

[0045] The plasticizing and molding steps are as follows: put the vacuum-exhausted material into a cooling agitator for cooling treatment, cool it to below 40°C, melt-extrude the mixed material on a twin-screw extruder, wherein the front section temperature of the twin-screw extruder is 80°C, the middle section temperature is 130°C, the rear section temperature is 150°C, and the head temperature is 80°C. The extruded material is granulated to obtain a polyvinyl chloride elastomer material.

[0046] The post-processing steps are as follows: (1) initial water cooling: water cooling of the polyvinyl chloride elastomer material is achieved through one or more water cooling tanks; (2) air cooling: after water cooling, the polyvinyl chloride elastomer material further passes through the air cooling zone of the fan to help the surface and interior of the material continue to cool down; (3) curing: the material is maintained below 80°C to ensure that it is fully cured.

[0047] Depend on Figure 2 It can be seen that when the plasticizer, nanomaterial and preparation conditions are consistent, the polyvinyl chloride elastomer material prepared in Example 3 with the addition of polyacrylate elastomer has a lower brittle temperature and better cold resistance.

[0048] Embodiment 4, an embodiment provided by the present invention: a process for preparing an environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators, comprising the following steps; S1, raw material preparation; S2, premixing; S3, melt blending; S4, plasticizing and molding; S5, post-processing.

[0049] The steps of preparing raw materials are as follows: by weight, prepare 100 parts of polyvinyl chloride resin, 70 parts of polyacrylate, 15 parts of nano-silicon dioxide, 20 parts of chlorinated paraffin plasticizer, 10 parts of calcium zinc composite stabilizer, 2 parts of lubricant, 0.5 parts of antioxidant and 0.5 parts of defoaming agent.

[0050] The premixing steps are as follows: premix polyvinyl chloride resin with polyacrylate, nano silicon dioxide, chlorinated paraffin plasticizer, calcium zinc composite stabilizer, lubricant, antioxidant and defoamer in a high-speed mixer to ensure that the raw materials are fully mixed evenly, the speed is 3000r / min, and the mixing power is controlled at 20KW.

[0051] The melt blending steps are as follows: add the pre-mixed raw materials into an internal mixer for melt blending, the blending temperature is 160°C, the blending time is 90min, the rotor speed is 60r / min, and in the molten state, the components are fully mixed and dispersed through shearing and mixing.

[0052] The plasticizing and molding steps are as follows: put the vacuum-exhausted material into a cooling agitator for cooling treatment, cool it to below 40°C, melt-extrude the mixed material on a twin-screw extruder, wherein the front section temperature of the twin-screw extruder is 80°C, the middle section temperature is 130°C, the rear section temperature is 150°C, and the head temperature is 80°C. The extruded material is granulated to obtain a polyvinyl chloride elastomer material.

[0053] The post-processing steps are as follows: (1) initial water cooling: water cooling of the polyvinyl chloride elastomer material is achieved through one or more water cooling tanks; (2) air cooling: after water cooling, the polyvinyl chloride elastomer material further passes through the air cooling zone of the fan to help the surface and interior of the material continue to cool down; (3) curing: the material is maintained below 80°C to ensure that it is fully cured.

[0054] Depend on Figure 2 It can be seen that when the nanomaterial, stabilizer and preparation conditions are consistent, the polyvinyl chloride elastomer material prepared in Example 4 using chlorinated paraffin as the plasticizer has a lower brittle temperature, fewer bubbles and cracks, and better cold resistance.

[0055] Embodiment 5, an embodiment provided by the present invention: a process for preparing an environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators, comprising the following steps; S1, raw material preparation; S2, premixing; S3, melt blending; S4, plasticizing and molding; S5, post-processing.

[0056] The steps of preparing raw materials are as follows: by weight, prepare 100 parts of polyvinyl chloride resin, 70 parts of polyacrylate, 15 parts of nano-silicon dioxide, 20 parts of chlorinated paraffin plasticizer, 10 parts of monoethyl ester, 10 parts of rare earth heat stabilizer, 2 parts of lubricant, 0.5 parts of antioxidant and 0.5 parts of defoamer.

[0057] The premixing steps are as follows: premix polyvinyl chloride resin with polyacrylate, nano-silica, chlorinated paraffin plasticizer, monoethyl ester, rare earth heat stabilizer, lubricant, antioxidant and defoamer in a high-speed mixer to ensure that the raw materials are fully mixed evenly, the speed is 3000r / min, and the mixing power is controlled at 20KW.

[0058] The melt blending steps are as follows: add the pre-mixed raw materials into an internal mixer for melt blending, the blending temperature is 160°C, the blending time is 90min, the rotor speed is 60r / min, and in the molten state, the components are fully mixed and dispersed through shearing and mixing.

[0059] The plasticizing and molding steps are as follows: put the vacuum-exhausted material into a cooling agitator for cooling treatment, cool it to below 40°C, melt-extrude the mixed material on a twin-screw extruder, wherein the front section temperature of the twin-screw extruder is 80°C, the middle section temperature is 130°C, the rear section temperature is 150°C, and the head temperature is 80°C. The extruded material is granulated to obtain a polyvinyl chloride elastomer material.

[0060] The post-processing steps are as follows: (1) initial water cooling: water cooling of the polyvinyl chloride elastomer material is achieved through one or more water cooling tanks; (2) air cooling: after water cooling, the polyvinyl chloride elastomer material further passes through the air cooling zone of the fan to help the surface and interior of the material continue to cool down; (3) curing: the material is maintained below 80°C to ensure that it is fully cured.

[0061] Depend on Figure 2 It can be seen that when the plasticizer, nanomaterial and preparation conditions are consistent, the waste gas emission of the polyvinyl chloride elastomer material prepared in Example 5 using a rare earth thermal stabilizer as the stabilizer is lower.

[0062] Embodiment 6, an embodiment provided by the present invention: a process for preparing an environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators, comprising the following steps; S1, raw material preparation; S2, premixing; S3, melt blending; S4, cross-linking reaction; S5, plasticizing and molding; S6, post-processing.

[0063] The steps of preparing raw materials are as follows: by weight, prepare 100 parts of polyvinyl chloride resin, 70 parts of polyacrylate, 15 parts of nano-silica, 20 parts of chlorinated paraffin plasticizer, 10 parts of monoethyl ester, 10 parts of rare earth heat stabilizer, 1 part of phenolic resin crosslinker, 2 parts of lubricant, 0.5 parts of antioxidant and 0.5 parts of defoamer.

[0064] The premixing steps are as follows: premix polyvinyl chloride resin with polyacrylate, nano-silica, chlorinated paraffin plasticizer, monoethyl ester, rare earth heat stabilizer, lubricant, antioxidant and defoamer in a high-speed mixer to ensure that the raw materials are fully mixed evenly, the speed is 3000r / min, and the mixing power is controlled at 20KW.

[0065] The melt blending steps are as follows: add the pre-mixed raw materials into an internal mixer for melt blending, the blending temperature is 160°C, the blending time is 90min, the rotor speed is 60r / min, and in the molten state, the components are fully mixed and dispersed through shearing and mixing.

[0066] The cross-linking reaction steps are as follows: adding a phenolic resin cross-linking agent to initiate a cross-linking reaction during melt blending, the blending temperature is 160° C., the blending time is 10 min, and the rotor speed is 60 r / min.

[0067] The plasticizing and molding steps are as follows: put the vacuum-exhausted material into a cooling agitator for cooling treatment, cool it to below 40°C, melt-extrude the mixed material on a twin-screw extruder, wherein the front section temperature of the twin-screw extruder is 80°C, the middle section temperature is 130°C, the rear section temperature is 150°C, and the head temperature is 80°C. The extruded material is granulated to obtain a polyvinyl chloride elastomer material.

[0068] The post-processing steps are as follows: (1) initial water cooling: water cooling of the polyvinyl chloride elastomer material is achieved through one or more water cooling tanks; (2) air cooling: after water cooling, the polyvinyl chloride elastomer material further passes through the air cooling zone of the fan to help the surface and interior of the material continue to cool down; (3) curing: the material is maintained below 80°C to ensure that it is fully cured.

[0069] Depend on Figure 2 It can be seen that when the plasticizer, nanomaterial and stabilizer are consistent, the polyvinyl chloride elastomer material prepared in Example 6 by adding phenolic resin for cross-linking reaction has a higher heat-resistant temperature and better heat-resistant performance.

[0070] Embodiment 7, an embodiment provided by the present invention: a process for preparing an environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators, comprising the following steps; S1, raw material preparation; S2, premixing; S3, melt blending; S4, cross-linking reaction; S5, vacuum exhaust; S6, plasticizing and molding; S7, post-processing.

[0071] The steps of preparing raw materials are as follows: by weight, prepare 100 parts of polyvinyl chloride resin, 70 parts of polyacrylate, 15 parts of nano-silica, 20 parts of chlorinated paraffin plasticizer, 10 parts of monoethyl ester, 10 parts of rare earth heat stabilizer, 1 part of phenolic resin crosslinker, 2 parts of lubricant, 0.5 parts of antioxidant and 0.5 parts of defoamer.

[0072] The premixing steps are as follows: premix polyvinyl chloride resin with polyacrylate, nano-silica, chlorinated paraffin plasticizer, monoethyl ester, rare earth heat stabilizer, lubricant, antioxidant and defoamer in a high-speed mixer to ensure that the raw materials are fully mixed evenly, the speed is 3000r / min, and the mixing power is controlled at 20KW.

[0073] The melt blending steps are as follows: add the pre-mixed raw materials into an internal mixer for melt blending, the blending temperature is 160°C, the blending time is 90min, the rotor speed is 60r / min, and in the molten state, the components are fully mixed and dispersed through shearing and mixing.

[0074] The cross-linking reaction steps are as follows: adding a phenolic resin cross-linking agent to initiate a cross-linking reaction during melt blending, the blending temperature is 160° C., the blending time is 10 min, and the rotor speed is 60 r / min.

[0075] The vacuum exhaust steps are as follows: after the material mixing is completed, the mixed material is transferred to the vacuum kneader, the exhaust port of the vacuum kneader is closed and the vacuum pump is started to evacuate the inside of the equipment. When the vacuum degree reaches -0.09MPa, it is maintained for 5 minutes to ensure that the bubbles in the material are fully extracted. After the exhaust is completed, the vacuum pump is closed and the exhaust port is opened to take out the material.

[0076] The plasticizing and molding steps are as follows: put the vacuum-exhausted material into a cooling agitator for cooling treatment, cool it to below 40°C, melt-extrude the mixed material on a twin-screw extruder, wherein the front section temperature of the twin-screw extruder is 80°C, the middle section temperature is 130°C, the rear section temperature is 150°C, and the head temperature is 80°C. The extruded material is granulated to obtain a polyvinyl chloride elastomer material.

[0077] The post-processing steps are as follows: (1) initial water cooling: water cooling of the polyvinyl chloride elastomer material is achieved through one or more water cooling tanks; (2) air cooling: after water cooling, the polyvinyl chloride elastomer material further passes through the air cooling zone of the fan to help the surface and interior of the material continue to cool down; (3) curing: the material is maintained below 80°C to ensure that it is fully cured.

[0078] Depend on Figure 2 It can be seen that when the plasticizer, nanomaterial and stabilizer are consistent, the polyvinyl chloride elastomer material prepared in Example 7 by vacuum exhaust has lower waste gas emissions and no bubble and crack defects.

[0079] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A preparation process of environmentally friendly cold-resistant polyvinyl chloride elastomer material for elevators. Features: The method comprises the following steps: S1, raw material preparation; S2, premixing; S3, melt blending; S4, cross-linking reaction; S5, vacuum exhaust; S6, plasticizing and molding; and S7, post-processing.

2. The preparation process of the environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators according to claim 1, Features: The raw material preparation steps are as follows: by weight, prepare 100 parts of polyvinyl chloride resin, 70-90 parts of polyacrylate, 15-30 parts of nano silicon dioxide, 20-25 parts of chlorinated paraffin plasticizer, 10-15 parts of monoethyl ester, 10-15 parts of rare earth heat stabilizer, 1-5 parts of phenolic resin crosslinker, 2-3 parts of lubricant, 0.5-1 part of antioxidant and 0.5-0.8 part of defoamer.

3. The preparation process of the environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators according to claim 2, Features: The polyvinyl chloride resin is prepared by adopting a low-temperature polymerization process, followed by washing, centrifugal dehydration and drying.

4. The process for preparing an environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators according to claim 2, Features: The premixing step is as follows: premixing polyvinyl chloride resin with polyacrylate, nano silicon dioxide, chlorinated paraffin plasticizer, monoethyl ester, rare earth heat stabilizer, lubricant, antioxidant and defoamer in a high-speed mixer to ensure that the raw materials are fully mixed and uniform, the rotation speed is 3000r / min, and the mixing power is controlled at 20-55KW.

5. The process for preparing the environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators according to claim 4, Features: The melt blending step is as follows: adding the premixed raw materials into an internal mixer for melt blending, the blending temperature is 160-180° C., the blending time is 60-90 min, the rotor speed is 40-60 r / min, and in the molten state, the components are fully mixed and dispersed through shearing and mixing.

6. The process for preparing the environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators according to claim 5, Features: The cross-linking reaction steps are as follows: adding a phenolic resin cross-linking agent during melt blending to initiate a cross-linking reaction, the blending temperature is 160-180° C., the blending time is 10-15 minutes, and the rotor speed is 40-60 r / min.

7. The process for preparing an environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators according to claim 6, Features: The vacuum exhaust step is as follows: after the material mixing is completed, the mixed material is transferred to the vacuum kneader, the exhaust port of the vacuum kneader is closed and the vacuum pump is started to evacuate the inside of the equipment. When the vacuum degree reaches -0.09MPa, it is maintained for 5 to 8 minutes to ensure that the bubbles in the material are fully extracted. After the exhaust is completed, the vacuum pump is closed and the exhaust port is opened to take out the material.

8. The process for preparing the environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators according to claim 7, Features: The plasticizing and molding steps are as follows: placing the vacuum-exhausted material into a cooling stirrer for cooling treatment, cooling to below 40°C, and melt-extrude the mixed material on a twin-screw extruder, wherein the front section temperature of the twin-screw extruder is 80-110°C, the middle section temperature is 130-150°C, the rear section temperature is 150-170°C, and the head temperature is 80-100°C. The extruded material is granulated to obtain a polyvinyl chloride elastomer material.

9. The process for preparing an environmentally friendly and cold-resistant polyvinyl chloride elastomer material for elevators according to claim 8, Features: The post-treatment steps are as follows: (1) preliminary water cooling: water cooling of the polyvinyl chloride elastomer material is achieved through one or more water cooling tanks; (2) air cooling: after water cooling, the polyvinyl chloride elastomer material further passes through the air cooling zone of the fan to help the surface and interior of the material continue to cool down; (3) curing: the material is maintained at 80-100°C to ensure that it is fully cured.

Citation Information

Patent Citations

  • Preparation method for dynamic cross-linking flame retardant chlorinated polyethylene thermoplastic elastomer

    CN102977479A

  • Dynamically vulcanized thermoplastic acrylate rubber composition and preparation method thereof

    CN108047595A

  • Polyvinyl chloride cable material and preparation method thereof

    CN109233145A

  • Cold-resistant polyvinyl chloride cable sheath material

    CN112194862A

  • High-toughness polyvinyl chloride steel framework plastic dipping liquid and plastic dipping method thereof

    CN113683844A