Light and thin down lining PUR bonding composite fabric and processing technology thereof
Through the design of the modified polymer network, the water-resistant and moisture-permeable properties of the light and thin down-lined composite fabric are improved, solving the problem of falling off between layers after washing, extending the service life and improving wear comfort.
Patent Information
- Application Number
- CN202410938453.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-13
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-13
AI Technical Summary
The light and thin down-lined composite fabric is prone to fall off between layers after washing, which affects the service life. The existing PUR glue has insufficient water-resistant performance.
PUR glue using modified polyether polycarbonate polyol, end amino crosslinking agent, fluorinated modified isocyanate and water-resistant modified chain extender to form a stable polymer through the crosslinking network and hydrophobic performance. Network, enhanced adhesion and wash resistance.
It significantly improves the washing resistance and moisture permeability of composite fabrics, extends service life, and improves the wear comfort of the fabric.
Smart Images

Figure CN118876515A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of composite fabrics, and in particular to a thin down-lined PUR bonded composite fabric and a processing technology thereof. Background Art
[0002] Down jackets are made by sewing animal feathers into clothes and are used for warmth in winter. They are widely loved by people because of their excellent warmth-keeping effect. However, due to the fluffy down, down jackets are large in size and appear bloated after wearing. In the central and southern regions where the temperature is suitable, the warmth-keeping effect of down jackets is better than the actual demand. Therefore, merchants make down jackets thinner and lighter so that they can be worn as linings. Conventional down products have the phenomenon of down coming out of the clothes or clumping after washing after long-term use. After long-term use, the down in the clothes becomes less and less or becomes less loose.
[0003] The thin down lining composite fabric uses glue to bond the down scraps between two layers of fabric, and then performs hot pressing bonding, which can effectively reduce the occurrence of down running and make the down evenly distributed in the fabric. PUR glue is a single-component moisture-curing polyurethane hot melt adhesive. It has the initial bonding speed of hot melt adhesive and the bonding strength of structural adhesive. After cooling, it can continue to cure for several hours to several days under ambient humidity conditions, and the strength continues to increase. However, the fabric will undergo several washings and cleanings, and the composite fabric is prone to interlayer shedding, which affects the service life, so it needs to be improved. Summary of the invention
[0004] In order to improve the washability of PUR glue, the present application provides a thin down lining PUR bonded composite fabric and a processing technology thereof.
[0005] The present application provides a lightweight down lining PUR bonded composite fabric and its processing technology using the following technical solutions: In the first aspect, the present application provides a thin down lining PUR bonded composite fabric, which adopts the following technical solution: a thin down lining PUR bonded composite fabric, the thin down lining PUR bonded composite fabric sequentially comprises a lower fabric, a glue-bonded down layer and an upper fabric, the glue-bonded down layer is bonded with PUR glue, and the PUR glue comprises the following components in parts by mass: Modified polyether polycarbonate polyol 30-40 parts 10-20 parts of amino-terminated crosslinking agent 20-30 parts of fluorinated modified isocyanate Water-resistant modified chain extender 5-8 parts Catalyst 0.1-0.2 parts.
[0006] Modified polyether polycarbonate polyol has good bonding properties and water washing resistance through modification treatment; terminal amino crosslinking agent has good reaction performance, and through crosslinking polymerization with the main chain of PUR glue molecules, a crosslinking network is formed to improve the stability of polymer molecules, thereby improving its water washing resistance; fluorinated modified isocyanate introduces fluorine element, which can improve the stability and hydrophobicity of PUR glue, thereby improving its water washing resistance; water-resistant modified chain extender can synergize with terminal amino crosslinking agent to further strengthen the crosslinking structure of the main chain of PUR glue molecules and improve its stability and water washing resistance.
[0007] Preferably, the raw materials for preparing the modified polyether polycarbonate polyol include carbon dioxide, maleopimaric anhydride and propylene oxide.
[0008] Preferably, the raw materials for preparing the maleopimaric anhydride include maleic anhydride and gum rosin.
[0009] Gum rosin has abundant active groups. Maleopimaric anhydride obtained by reacting with maleic anhydride has good reaction performance and bonding performance. Introducing maleopimaric anhydride as a functional monomer into the synthesis of polyether polycarbonate can effectively improve the adhesion performance and reaction activity of modified polyether polycarbonate polyols, reduce the adsorption of water by PUR glue, improve the hydrophobicity, thereby reducing the performance degradation caused by water erosion, and improving its stability and water washability.
[0010] Preferably, the raw materials for preparing the amino-terminated cross-linking agent include 1,3-propylenediamine and methylguanamine.
[0011] The terminal amino cross-linking agent generated by the reaction of methylguanamine and 1,3-propylenediamine has high reactivity and active amino groups at both ends of the molecule. It can be effectively grafted onto the molecular main chain of PUR glue to form an orderly and controllable branched structure. While improving the water-washing resistance of the composite fabric, the glue-bonded down layer retains a good pore structure, so that the composite fabric can have good water-washing resistance while having good moisture permeability, thereby improving the wearing comfort of the fabric.
[0012] Preferably, the raw materials for preparing the fluorinated modified isocyanate include isocyanate and a fluorinated grafting agent.
[0013] Preferably, the fluorinated grafting agent comprises 3-(aminomethyl)-5-fluorophenol.
[0014] 3-(Aminomethyl)-5-fluorophenol introduces benzene ring structure and fluorine atom into isocyanate molecules, thereby improving the hydrophobicity and stability of isocyanate and reducing its surface energy, thereby improving its water wash resistance. 3-(Aminomethyl)-5-fluorophenol introduces more active groups into the isocyanate molecules, which can form multiple chemical bonds such as hydrogen bonds between the layers of composite fabrics, thereby giving the composite fabrics a strong binding force and enhancing the adhesion performance.
[0015] Preferably, the mass ratio of the isocyanate to the fluorinated grafting agent is 1:(0.6-0.8).
[0016] The fluorinated modified isocyanate prepared according to the above mass ratio can improve the bonding performance and water washability of PUR glue.
[0017] Preferably, the water-resistant modified chain extender includes tannic acid and 1,10-diaminodecane.
[0018] Tannic acid molecules have rich catechol structures, which can improve the adhesion performance of glue; the water-resistant modified chain extender obtained by the reaction of tannic acid and 1,10-diaminodecane can successfully introduce tannic acid into the side chain of PUR glue molecules, reduce the influence of steric hindrance on the reaction, and transform simple blending into graft copolymerization. The phenolic hydroxyl group of tannic acid molecules can also react with fluorinated modified isocyanate, so that the water-resistant modified chain extender and the terminal amino cross-linking agent work synergistically to construct a stable polymer network; the structure of tannic acid can also effectively control the occurrence of chain extension reaction, thereby regulating the pore structure, so that the composite fabric can maintain good moisture permeability.
[0019] Preferably, the mass ratio of tannic acid to 1,10-diaminodecane is 1:(0.2-0.3).
[0020] The water-resistant modified chain extender prepared according to the above mass ratio has good reaction performance, can improve the bonding performance of the adhesive, and improve the water-resistant performance and moisture permeability of the composite fabric.
[0021] In the second aspect, the present application provides a processing technology for a thin down lining PUR bonding composite fabric, which adopts the following technical solution: A processing technology for bonding PUR composite fabrics for thin down linings, comprising the following steps: Modified polyether polycarbonate polyol, fluorinated modified isocyanate, water-resistant modified chain extender and catalyst are mixed and dispersed to obtain a prepolymer mixture, the prepolymer mixture is heated to react, and an amino-terminated cross-linking agent is added to the prepolymer mixture after the reaction, and the heating reaction is continued to obtain PUR glue after cooling; down crumbs are evenly laid on the lower fabric, and glue is applied to the lower fabric after the down is laid to obtain a glue-bonded down layer, and the upper fabric is hot-pressed and bonded to the glue-bonded down layer to obtain a thin down lining PUR bonded composite fabric.
[0022] The composite fabric prepared according to the above steps has good water wash resistance, stability and moisture permeability.
[0023] In summary, the present application includes at least one of the following beneficial technical effects: 1. The modified polyether polycarbonate polyol has good bonding properties and water washing resistance through modification. The terminal amino crosslinker has good reaction performance and forms a crosslinking network through crosslinking polymerization with the main chain of PUR glue molecules, thereby improving the stability of polymer molecules and thus improving its water washing resistance. The fluorinated modified isocyanate introduces fluorine elements, which can improve the stability and hydrophobicity of PUR glue, thereby improving its water washing resistance. The water-resistant modified chain extender can synergize with the terminal amino crosslinker to further strengthen the crosslinking structure of the main chain of PUR glue molecules and improve its stability and water washing resistance.
[0024] 2. The terminal amino cross-linking agent generated by the reaction of methylguanamine and 1,3-propylenediamine has high reactivity and active amino groups at both ends of the molecule. It can be effectively grafted onto the molecular main chain of PUR glue to form an orderly and controllable branched structure. While improving the water-washing resistance of the composite fabric, the glue-bonded down layer retains a good pore structure, so that the composite fabric can have good water-washing resistance while having good moisture permeability, thereby improving the wearing comfort of the fabric.
[0025] 3. Tannic acid molecules have rich catechol structures, which can improve the adhesion performance of glue; the water-resistant modified chain extender obtained by the reaction of tannic acid and 1,10-diaminodecane can successfully introduce tannic acid into the side chain of PUR glue molecules, reduce the influence of steric hindrance on the reaction, and transform simple blending into graft copolymerization. The phenolic hydroxyl group of tannic acid molecules can also react with fluorinated modified isocyanate, so that the water-resistant modified chain extender and the terminal amino cross-linking agent work synergistically to construct a stable polymer network; the structure of tannic acid can also effectively control the occurrence of chain extension reaction, thereby regulating the pore structure, so that the composite fabric can maintain good moisture permeability. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a cross-sectional view of a thin down lining PUR bonded composite fabric in an embodiment of the present application.
[0027] Description of the accompanying drawings: 1. Upper fabric layer; 2. Glue-bonded down layer; 3. Lower fabric layer. DETAILED DESCRIPTION
[0028] The embodiment of the present application discloses a light and thin down lining PUR bonded composite fabric and its processing technology. The raw materials used in the present application can be obtained through commercially available raw materials unless otherwise specified. The present application is further described in detail in combination with the embodiments below: Raw material description: gum rosin (CAS No.: 8050-09-7), maleic anhydride (CAS No.: 108-31-6), dibutyltin dilaurate (CAS No.: 77-58-7), turpentine (CAS No.: 8006-64-2), propylene oxide (CAS No.: 75-56-9), bis(triphenylphosphorane)ammonium chloride (CAS No.: 21050-13-5), triethyl boron (CAS No.: 97-94-9), 1,3-propylenediamine (CAS No.: 1 09-76-2), methylguanamine (CAS No.: 542-02-9), isocyanate is isophorone diisocyanate (CAS No.: 4098-71-9), fluorinated grafting agent is 3-(aminomethyl)-5-fluorophenol (CAS No.: 1243285-06-4), tannic acid (CAS No.: 1401-55-4), 1,10-diaminodecane (CAS No.: 646-25-3), catalyst is dibutyltin dilaurate, fluorinated polyol is pentafluoro-1-propanol (CAS No.: 422-05-9), ethylenediamine (CAS No.: 107-15-3), polyether polyol (CAS No.: 9003-11-6), aziridine (CAS No.: 151-56-4).
[0029] Example 1 Preparation of modified polyether polycarbonate polyols 15.1 kg of gum rosin, 2.88 kg of maleic anhydride and 0.3 kg of dibutyltin dilaurate were mixed and dispersed, ammonia was introduced for 15 minutes, and then the material was heated to melt, then stirred at a speed of 200 rpm and heated to 180°C. After reacting at 180°C for 4 hours, the product was cooled to 110°C and poured into turpentine oil, crystallized at room temperature, and the crystals were filtered and washed with ethanol for 3 times. The washed crystals were dried in a vacuum oven at 60°C to obtain maleopimaric anhydride.
[0030] In a dry environment, 4.5 kg of maleopimaric anhydride and 45 kg of propylene oxide were mixed and dispersed, 15 g of bis(triphenylphosphorane)ammonium chloride and 36 g of triethylboron were added to obtain a mixed reaction system, the mixed reaction system was heated to 70° C. and reacted for 2.5 hours, the mixed reaction system was cooled in 20° C. water for 5 minutes, 3 g of triethylboron was added to the mixed reaction system, and carbon dioxide was introduced to maintain the pressure at 4 MPa, the mixed reaction system was reacted at 50° C. for 7 hours, and then cooled in an ice water bath, 1 mol / L hydrochloric acid was added to quench the reaction to obtain a crude product, the crude product was dissolved in dichloromethane, precipitated in ethanol, and the obtained precipitate was dried in a vacuum oven at 80° C. to obtain a modified polyether polycarbonate polyol, which was stored in a dry environment for later use.
[0031] Preparation of amino-terminated crosslinkers 11.25 kg of 1,3-propylenediamine and 18.75 kg of methylguanamine were mixed and dispersed in 50 L of acetone, and 1 kg of ammonium chloride was added to obtain a crosslinker reaction solution. The crosslinker reaction solution was heated to 80° C. and reacted for 2 h. After rotary evaporation, it was washed with deionized water and dried in an oven at 60° C. to obtain an amino-terminated crosslinker.
[0032] Preparation of fluorinated modified isocyanates 31.25 kg of isocyanate was dispersed in 50 L of ethyl acetate to obtain an isocyanate solution, 18.75 kg of fluorinated grafting agent was dispersed in 30 L of ethyl acetate to obtain a grafting agent solution, 0.1 kg of dibutyltin dilaurate was used as a catalyst, and the grafting agent solution was added to the isocyanate solution within 30 min. The reaction was stirred at 40 ° C for 2 h in a nitrogen atmosphere with a stirring speed of 200 rpm. After reduced pressure distillation, it was cooled to below 30 ° C to obtain a fluorinated modified isocyanate.
[0033] Preparation of hydrophobically modified chain extenders 8.33 kg of tannic acid and 20 L of 0.01 mol / L hydrochloric acid were mixed and stirred to obtain a tannic acid solution, 1.67 kg of 1,10-diaminodecane was dispersed in ethanol to obtain an ammonia solution, the ammonia solution was added to the tannic acid solution, and the mixture was stirred at 200 rpm in a water bath at 80°C for 4 hours, and then dried in an oven at 60°C after rotary evaporation to obtain a hydrophobically modified chain extender.
[0034] Preparation of lightweight down-lined PUR bonded composite fabric 30kg of modified polyether polycarbonate polyol, 20kg of fluorinated modified isocyanate, 5kg of water-resistant modified chain extender and 0.1kg of catalyst are mixed and dispersed to obtain a prepolymer mixture, the prepolymer mixture is heated to 80°C and reacted for 6h, 10kg of terminal amino cross-linking agent is added to the prepolymer mixture after the reaction, and the reaction is continued at 80°C for 2h, and PUR glue is obtained after cooling to 30°C; down crumbs are evenly laid on the lower fabric, glue is applied to the lower fabric after the down is laid to obtain a glue-bonded down layer, the upper fabric is bonded to the glue-bonded down layer, hot pressing is performed at 90°C, and the fabric is placed under 50% humidity for 3d to obtain a thin down lining PUR bonded composite fabric.
[0035] Example 2 Preparation of modified polyether polycarbonate polyols 15.1 kg of gum rosin, 2.88 kg of maleic anhydride and 0.3 kg of dibutyltin dilaurate were mixed and dispersed, ammonia was introduced for 15 minutes, and then the material was heated to melt, then stirred at a speed of 200 rpm and heated to 180°C. After reacting at 180°C for 4 hours, the product was cooled to 110°C and poured into turpentine oil, crystallized at room temperature, and the crystals were filtered and washed with ethanol for 3 times. The washed crystals were dried in a vacuum oven at 60°C to obtain maleopimaric anhydride.
[0036] In a dry environment, 4.5 kg of maleopimaric anhydride and 45 kg of propylene oxide were mixed and dispersed, 15 g of bis(triphenylphosphorane)ammonium chloride and 36 g of triethylboron were added to obtain a mixed reaction system, the mixed reaction system was heated to 70° C. and reacted for 2.5 hours, the mixed reaction system was cooled in 20° C. water for 5 minutes, 3 g of triethylboron was added to the mixed reaction system, and carbon dioxide was introduced to maintain the pressure at 4 MPa, the mixed reaction system was reacted at 50° C. for 7 hours, and then cooled in an ice water bath, 1 mol / L hydrochloric acid was added to quench the reaction to obtain a crude product, the crude product was dissolved in dichloromethane, precipitated in ethanol, and the obtained precipitate was dried in a vacuum oven at 80° C. to obtain a modified polyether polycarbonate polyol, which was stored in a dry environment for later use.
[0037] Preparation of amino-terminated crosslinkers 11.25 kg of 1,3-propylenediamine and 18.75 kg of methylguanamine were mixed and dispersed in 50 L of acetone, and 1 kg of ammonium chloride was added to obtain a crosslinker reaction solution. The crosslinker reaction solution was heated to 80° C. and reacted for 2 h. After rotary evaporation, it was washed with deionized water and dried in an oven at 60° C. to obtain an amino-terminated crosslinker.
[0038] Preparation of fluorinated modified isocyanates 27.78 kg of isocyanate was dispersed in 50 L of ethyl acetate to obtain an isocyanate solution, 22.22 kg of fluorinated grafting agent was dispersed in 30 L of ethyl acetate to obtain a grafting agent solution, 0.1 kg of dibutyltin dilaurate was used as a catalyst, and the grafting agent solution was added to the isocyanate solution within 30 min. The reaction was stirred at 40 ° C for 2 h in a nitrogen atmosphere with a stirring speed of 200 rpm. After reduced pressure distillation, it was cooled to below 30 ° C to obtain a fluorinated modified isocyanate.
[0039] Preparation of hydrophobically modified chain extenders 7.69 kg of tannic acid and 20 L of 0.01 mol / L hydrochloric acid were mixed and stirred to obtain a tannic acid solution, 2.31 kg of 1,10-diaminodecane was dispersed in ethanol to obtain an ammonia solution, the ammonia solution was added to the tannic acid solution, and the mixture was stirred at 200 rpm in a water bath at 80°C for 4 hours, and then dried in an oven at 60°C after rotary evaporation to obtain a hydrophobically modified chain extender.
[0040] Preparation of lightweight down-lined PUR bonded composite fabric 40 kg of modified polyether polycarbonate polyol, 30 kg of fluorinated modified isocyanate, 8 kg of water-resistant modified chain extender and 0.2 kg of catalyst are mixed and dispersed to obtain a prepolymer mixture, the prepolymer mixture is heated to 80°C and reacted for 6 hours, 20 kg of terminal amino cross-linking agent is added to the prepolymer mixture after the reaction, and the reaction is continued at 80°C for 2 hours, and PUR glue is obtained after cooling to 30°C; down crumbs are evenly laid on the lower fabric, glue is applied to the lower fabric after the down is laid to obtain a glue-bonded down layer, the upper fabric is bonded to the glue-bonded down layer, hot pressing is performed at 90°C, and the fabric is placed under 50% humidity for 3 days to obtain a thin down lining PUR bonded composite fabric.
[0041] Example 3 Preparation of modified polyether polycarbonate polyols 15.1 kg of gum rosin, 2.88 kg of maleic anhydride and 0.3 kg of dibutyltin dilaurate were mixed and dispersed, ammonia was introduced for 15 minutes, and then the material was heated to melt, then stirred at a speed of 200 rpm and heated to 180°C. After reacting at 180°C for 4 hours, the product was cooled to 110°C and poured into turpentine oil, crystallized at room temperature, and the crystals were filtered and washed with ethanol for 3 times. The washed crystals were dried in a vacuum oven at 60°C to obtain maleopimaric anhydride.
[0042] In a dry environment, 4.5 kg of maleopimaric anhydride and 45 kg of propylene oxide were mixed and dispersed, 15 g of bis(triphenylphosphorane)ammonium chloride and 36 g of triethylboron were added to obtain a mixed reaction system, the mixed reaction system was heated to 70° C. and reacted for 2.5 hours, the mixed reaction system was cooled in 20° C. water for 5 minutes, 3 g of triethylboron was added to the mixed reaction system, and carbon dioxide was introduced to maintain the pressure at 4 MPa, the mixed reaction system was reacted at 50° C. for 7 hours, and then cooled in an ice water bath, 1 mol / L hydrochloric acid was added to quench the reaction to obtain a crude product, the crude product was dissolved in dichloromethane, precipitated in ethanol, and the obtained precipitate was dried in a vacuum oven at 80° C. to obtain a modified polyether polycarbonate polyol, which was stored in a dry environment for later use.
[0043] Preparation of amino-terminated crosslinkers 11.25 kg of 1,3-propylenediamine and 18.75 kg of methylguanamine were mixed and dispersed in 50 L of acetone, and 1 kg of ammonium chloride was added to obtain a crosslinker reaction solution. The crosslinker reaction solution was heated to 80° C. and reacted for 2 h. After rotary evaporation, it was washed with deionized water and dried in an oven at 60° C. to obtain an amino-terminated crosslinker.
[0044] Preparation of fluorinated modified isocyanates 29.41 kg of isocyanate was dispersed in 50 L of ethyl acetate to obtain an isocyanate solution, 20.59 kg of fluorinated grafting agent was dispersed in 30 L of ethyl acetate to obtain a grafting agent solution, 0.1 kg of dibutyltin dilaurate was used as a catalyst, and the grafting agent solution was added to the isocyanate solution within 30 min. The reaction was stirred at 40 ° C for 2 h in a nitrogen atmosphere with a stirring speed of 200 rpm. After reduced pressure distillation, it was cooled to below 30 ° C to obtain a fluorinated modified isocyanate.
[0045] Preparation of hydrophobically modified chain extenders 8 kg of tannic acid and 20 L of 0.01 mol / L hydrochloric acid were mixed and stirred to obtain a tannic acid solution, 2 kg of 1,10-diaminodecane was dispersed in ethanol to obtain an ammonia solution, the ammonia solution was added to the tannic acid solution, and the mixture was stirred at 200 rpm in a water bath at 80°C for 4 hours, and then dried in an oven at 60°C after rotary evaporation to obtain a hydrophobically modified chain extender.
[0046] Preparation of lightweight down-lined PUR bonded composite fabric 35 kg of modified polyether polycarbonate polyol, 25 kg of fluorinated modified isocyanate, 6.5 kg of water-resistant modified chain extender and 0.15 kg of catalyst are mixed and dispersed to obtain a prepolymer mixture, the prepolymer mixture is heated to 80°C and reacted for 6 hours, 15 kg of terminal amino cross-linking agent is added to the prepolymer mixture after the reaction, and the reaction is continued at 80°C for 2 hours, and PUR glue is obtained after cooling to 30°C; down crumbs are evenly laid on the lower fabric, glue is applied to the lower fabric after the down is laid to obtain a glue-bonded down layer, the upper fabric is bonded to the glue-bonded down layer, hot pressing is performed at 90°C, and the fabric is placed under 50% humidity for 3 days to obtain a thin down lining PUR bonded composite fabric.
[0047] Example 4 Example 4 is based on Example 3. The only difference between Example 4 and Example 3 is that maleopimaric anhydride is replaced by maleic anhydride when preparing the modified polyether polycarbonate polyol in Example 4.
[0048] Example 5 Example 5 is based on Example 3. The only difference between Example 5 and Example 3 is that in Example 5, the fluorinated grafting agent is replaced by a fluorinated polyol when preparing the fluorinated modified isocyanate.
[0049] Example 6 Example 6 is based on Example 3. The only difference between Example 6 and Example 3 is that in Example 6, the amount of isocyanate used is 33.33 kg, and the amount of fluorinated grafting agent used is 16.67 kg.
[0050] Example 7 Example 7 is based on Example 3. The only difference between Example 7 and Example 3 is that in Example 7, the amount of isocyanate used is 26.32 kg, and the amount of fluorinated grafting agent used is 23.68 kg.
[0051] Example 8 Example 8 is based on Example 3. The only difference between Example 8 and Example 3 is that in Example 8, 1,10-diaminosilane is replaced by ethylenediamine when preparing the water-resistant modified chain extender.
[0052] Example 9 Example 9 is based on Example 3. The only difference between Example 9 and Example 3 is that in Example 9, the amount of tannic acid used is 8.7 kg, and the amount of 1,10-diaminodecane used is 1.3 kg.
[0053] Example 10 Example 10 is based on Example 3. The only difference between Example 10 and Example 3 is that in Example 10, the amount of tannic acid used is 7.41 kg, and the amount of 1,10-diaminodecane used is 2.59 kg.
[0054] Comparative Example 1 Comparative Example 1 is based on Example 3, and the only difference between Comparative Example 1 and Example 3 is that in Comparative Example 1, the modified polyether polycarbonate polyol is replaced by polyether polyol.
[0055] Comparative Example 2 Comparative Example 2 is based on Example 3, and the only difference between Comparative Example 2 and Example 3 is that the amino-terminated cross-linking agent in Comparative Example 2 is replaced by aziridine.
[0056] Comparative Example 3 Comparative Example 3 is based on Example 3, and the only difference between Comparative Example 3 and Example 3 is that in Comparative Example 3, the fluorinated modified isocyanate is replaced by isophorone diisocyanate.
[0057] Comparative Example 4 Comparative Example 4 is based on Example 3, and the only difference between Comparative Example 4 and Example 3 is that in Comparative Example 4, the water-resistant modified chain extender is replaced by tannic acid.
[0058] Comparative Example 5 Comparative Example 5 is based on Example 3, and the only difference between Comparative Example 5 and Example 3 is that in Comparative Example 5, the water-resistant modified chain extender is replaced by 1,10-diaminodecane.
[0059] Performance testing (1) GB / T2792-2014 Test method for peel strength of adhesive tape was selected as the standard. The peel strength of the composite fabric was tested using a desktop tensile testing machine. The peel strength was tested before washing and after washing 30 times. Three samples were prepared for each sample. The average value was taken after measurement and the results were recorded in Table 1.
[0060] (2) Select "GB / T12704.2-2009 Test method for water vapor permeability of textile fabrics Part 2: Evaporation method" as the standard, cut three samples with a diameter of 70 cm from the composite fabric, and calculate the water vapor permeability of the samples by the inverted cup method under the conditions of temperature 38°C and humidity 50%. After measurement, take the average value of the three samples and fill in the measurement results in Table 1.
[0061] Table 1 Test results of bonding performance, water washability and moisture permeability of composite fabrics As shown in Table 1, the peeling force of Examples 1-3 before washing is greater than 24.7 N / 25 mm, the peeling force after washing is greater than 22.3 N / 25 mm, and the moisture permeability is greater than 8314 g / (m 2 · 24h), thus it can be seen that the composite fabric prepared in the present application has good adhesion, water washability and moisture permeability.
[0062] As can be seen from Table 1, the only difference between Example 4 and Example 3 is that maleopimaric anhydride is replaced by maleic anhydride when preparing the modified polyether polycarbonate polyol in Example 4. Compared with Example 3, the adhesion performance, water washing resistance and moisture permeability of Example 4 are all reduced. This is because maleopimaric anhydride is replaced by maleic anhydride, and there is a lack of modification treatment of gum rosin, the active groups of maleic anhydride are reduced, the reactivity and adhesion performance are reduced, the hydrophobicity is reduced, and the ability to resist water erosion is weakened, so that the adhesion performance, water washing resistance and moisture permeability of the composite fabric are all reduced.
[0063] As can be seen from Table 1, the only difference between Example 5 and Example 3 is that when preparing the fluorinated modified isocyanate in Example 5, the fluorinated grafting agent is replaced by a fluorinated polyol. Compared with Example 3, Example 5 has reduced adhesion and water wash resistance. This is because the grafting agent is replaced by a fluorinated polyol, the number of active groups of the fluorinated polyol is reduced, and the ability to form chemical bonds is weakened, thereby reducing the interlayer bonding force of the composite fabric. In addition, due to the lack of a benzene ring structure, the stability and hydrophobicity are also reduced, thereby reducing the adhesion and water wash resistance.
[0064] As can be seen from Table 1, the only difference between Examples 6 and 7 and Example 3 is that the mass ratio of isocyanate to fluorinated grafting agent in Example 6 is 1:0.5, and the mass ratio of isocyanate to fluorinated grafting agent in Example 7 is 1:0.9. Compared with Example 3, the adhesion performance and water washing resistance of Examples 6 and 7 are both reduced. This is because the mass ratio of isocyanate to fluorinated grafting agent is not within the specified range. Too much or too little fluorinated grafting agent will affect the reactivity of fluorinated modified isocyanate and the overall chemical bonding, thereby reducing the adhesion performance and water washing resistance.
[0065] As can be seen from Table 1, the only difference between Example 8 and Example 3 is that in Example 8, 1,10-diaminosilane is replaced by ethylenediamine when preparing the water-resistant modified chain extender. Compared with Example 3, Example 8 has reduced adhesion, water-washing resistance and moisture permeability. This is because 1,10-diaminosilane is replaced by ethylenediamine, the chain structure of ethylenediamine is short, and there is a large steric hindrance between tannic acid molecules. The reaction performance of the chain extender obtained by reacting with ethylenediamine is reduced, which in turn affects the cross-linking performance of the water-resistant modified chain extender. The synergistic effect of the water-resistant modified chain extender and the terminal amino cross-linking agent is weakened, so that the adhesion performance, water-washing resistance and moisture permeability are reduced.
[0066] As can be seen from Table 1, the only difference between Examples 9 and 10 and Example 3 is that the mass ratio of tannic acid to 1,10-diaminodecane in Example 9 is 1:0.15, and the mass ratio of tannic acid to 1,10-diaminodecane in Example 10 is 1:0.35. Compared with Example 3, the adhesion performance, water wash resistance and moisture permeability of Examples 9 and 10 are reduced. This is because the mass ratio of tannic acid to 1,10-diaminosilane is not within the specified range. Too much or too little 1,10-diaminodecane will affect the reaction performance and structure of the modified water-resistant modified chain extender, and then affect the morphology and stability of the polymer network, so that the adhesion performance, water wash resistance and moisture permeability are reduced.
[0067] As can be seen from Table 1, the only difference between Comparative Example 1 and Example 3 is that the modified polyether polycarbonate polyol is replaced by polyether polyol in Comparative Example 1. Compared with Example 3, the adhesion performance, water washing resistance and moisture permeability of Comparative Example 1 are significantly reduced. This is because the polyether polyol lacks the polycarbonate structure and the introduction of maleopimaric anhydride, the adhesion performance and hydrophobicity are reduced, the reaction activity is reduced, and the ability to resist moisture erosion is weakened, so that the adhesion performance, water washing resistance and moisture permeability are significantly reduced.
[0068] As can be seen from Table 1, the only difference between Comparative Example 2 and Example 3 is that: in Comparative Example 2, the terminal amino cross-linking agent is replaced by aziridine. Compared with Example 3, the adhesion performance, water wash resistance and moisture permeability of Comparative Example 2 are significantly reduced; this is because the terminal amino cross-linking agent is replaced by aziridine, the reaction activity of aziridine is weaker, the regulating effect on the pore structure is reduced, the stability of the PUR glue is reduced, and thus the adhesion performance, water wash resistance and moisture permeability are significantly reduced.
[0069] As can be seen from Table 1, the only difference between Comparative Example 3 and Example 3 is that: Comparative Example 3 replaces the fluorinated modified isocyanate with isophorone diisocyanate. Compared with Example 3, the adhesion performance, water wash resistance and moisture permeability of Comparative Example 3 are significantly reduced. This is because the surface energy of the glue molecules increases, the hydrophobic property decreases, and the stability is weakened due to the lack of modification treatment of 3-(aminomethyl)-5-fluorophenol. In addition, the chemical bonding effect is reduced due to the lack of introduction of active groups, so that the adhesion performance, water wash resistance and moisture permeability are significantly reduced.
[0070] As can be seen from Table 1, the only difference between Comparative Examples 4 and 5 and Example 3 is that: Comparative Example 4 replaces the water-resistant modified chain extender with tannic acid, and Comparative Example 5 replaces the water-resistant modified chain extender with 1,10-diaminodecane. Compared with Example 3, Comparative Examples 4 and 5 have significantly reduced adhesion, water-washing resistance and moisture permeability. This is because the water-resistant modified chain extender is replaced by tannic acid or 1,10-diaminodecane, tannic acid lacks diamine modification, and the reaction performance is reduced, 1,10-diaminodecane lacks catechol structure, the adhesion performance is reduced, the control of the chain extension reaction is weakened, and the pore structure is reduced, so that the adhesion performance, water-washing resistance and moisture permeability are significantly reduced.
[0071] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A thin down-lined PUR bonding composite fabric, Features: The thin down lining PUR bonded composite fabric comprises a lower fabric layer, a glue bonded down layer and an upper fabric layer in sequence, the glue bonded down layer is bonded with PUR glue, and the PUR glue comprises the following components in parts by mass: Modified polyether polycarbonate polyol 30-40 parts 10-20 parts of amino-terminated crosslinking agent 20-30 parts of fluorinated modified isocyanate Water-resistant modified chain extender 5-8 parts Catalyst 0.1-0.2 parts.
2. A thin down lining PUR bonding composite fabric according to claim 1, Features: The raw materials for preparing the modified polyether polycarbonate polyol include carbon dioxide, maleopimaric anhydride and propylene oxide.
3. A thin down lining PUR bonding composite fabric according to claim 2, Features: The raw materials for preparing the maleopimaric anhydride include maleic anhydride and gum rosin.
4. The thin down lining PUR bonding composite fabric according to claim 1, Features: The raw materials for preparing the terminal amino cross-linking agent include 1,3-propylenediamine and methylguanamine.
5. The thin down lining PUR bonding composite fabric according to claim 1, Features: The raw materials for preparing the fluorinated modified isocyanate include isocyanate and a fluorinated grafting agent.
6. A thin down lining PUR bonding composite fabric according to claim 5, Features: The fluorinated grafting agent includes 3-(aminomethyl)-5-fluorophenol.
7. A thin down-lined PUR bonded composite fabric according to claim 6, Features: The mass ratio of the isocyanate to the fluorinated grafting agent is 1:(0.6-0.8).
8. The thin down-lined PUR bonding composite fabric according to claim 1, Features: The water-resistant modified chain extender includes tannic acid and 1,10-diaminodecane.
9. The thin down-lined PUR bonding composite fabric according to claim 8, Features: The mass ratio of the tannic acid to 1,10-diaminodecane is 1:(0.2-0.3).
10. A processing technology for the thin down lining PUR bonding composite fabric as claimed in claim 1, Features: Use the following steps: Modified polyether polycarbonate polyol, fluorinated modified isocyanate, water-resistant modified chain extender and catalyst are mixed and dispersed to obtain a prepolymer mixture, the prepolymer mixture is heated to react, and an amino-terminated cross-linking agent is added to the prepolymer mixture after the reaction, and the heating reaction is continued to obtain PUR glue after cooling; down crumbs are evenly laid on the lower fabric, and glue is applied to the lower fabric after the down is laid to obtain a glue-bonded down layer, and the upper fabric is hot-pressed and bonded to the glue-bonded down layer to obtain a thin down lining PUR bonded composite fabric.
Citation Information
Patent Citations
Polyurethane dispersions for coating textiles
CN104066760A
PUR adhesive for garment materials and preparation method of PUR adhesive
CN115584235A
Reactive moisture-curable polyurethane hot melt adhesive as well as preparation method and application thereof
CN115926715A
Down feather fabric and preparation process thereof
CN116945705A
Cited By
High-temperature-resistant hot melt adhesive film and preparation method thereof
CN120888250A