Method for purifying iron phosphate source
By using ammonia water to adjust pH and add reducing iron powder in the iron phosphate source purification process, the problems of high cost, large safety hazards and poor reaction effect in the prior art are solved, and economical and efficient iron phosphate are achieved Iron source preparation saves 50-70 yuan in preparation cost.
Patent Information
- Application Number
- CN202410914759.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
AI Technical Summary
The existing iron phosphate purification process has high costs, high safety hazards and impurities introduced, and the economic cost control of the double iron source synthesis method is limited and the reaction effect is poor, resulting in high preparation cost and low efficiency.
Ferrous sulfate heptahydrate and raw water solution were prepared at 1:1.5, ammonia water was used to adjust the pH to 2.8-3.3, and then allowed to stand for half an hour and added reduced iron powder to 3.5-4.5. After reaction for 20 minutes, filtered to achieve iron ferrous phosphate source Purification.
This method reduces costs, shortens reaction time, improves reaction effect, avoids the problem of difficult separation of liquid and solids, saves preparation costs of 50-70 yuan per ton of iron phosphate, and the product quality is close to all iron powder.
Smart Images

Figure CN118877848A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron phosphate iron source treatment, and in particular to a method for purifying an iron phosphate iron source. Background Art
[0002] Currently, ferrous sulfate, a by-product of titanium dioxide, is used as an iron source. The contents of Mg, Mn and Ti are generally high. The more mature processes currently use high-purity reduced iron powder with an elemental iron content of ≥ 97% for purification, which is costly. The market for iron phosphate is currently sluggish, and product prices are not optimistic. It is a general trend to find a way to produce low-cost raw materials.
[0003] In the traditional method of preparing ferric phosphate from scrap iron, strong acids such as sulfuric acid, hydrochloric acid or nitric acid are usually used to directly dissolve the scrap iron to generate a soluble iron salt solution, which is then used to make ferric phosphate. The disadvantages of this method are that the acid used is a highly corrosive acid, which is prone to safety accidents during the dissolution process, and the cost of the acid is high. For example, 1 ton of pure iron needs to be dissolved with 5 tons of concentrated sulfuric acid, and a large amount of alkali is needed in the subsequent process to neutralize its strong acidity, which greatly increases its preparation cost. In addition, new impurity ions will be introduced.
[0004] After repeated verification in the laboratory, it was found that ammonia water can be used to replace part of the reduced iron powder. After dissolving the ferrous sulfate, a by-product of titanium dioxide, the pH can be adjusted in stages. At the same time, if all ammonia water is used to replace the reduced iron powder, the liquid and solid will be difficult to separate. Dissolve the ferrous sulfate at a ratio of 1:1.5, with an initial pH between 1.8-2.2. First use ammonia water to adjust the pH of the ferrous solution to 2.8-3.3, react for half an hour without separation, and then use reduced iron powder to adjust the pH to 3.5-4.5. React for 20 minutes and filter.
[0005] According to a preparation method for synthesizing iron phosphate using a dual iron source mentioned in the invention of Chinese patent application No. 202111368935.1, the preparation method for synthesizing iron phosphate using a dual iron source has the advantages of low impurity content, good electrical properties, and simple preparation process steps. However, the preparation method for synthesizing iron phosphate using a dual iron source has limited control over economic costs, which is not conducive to cost control. In addition, through the preparation method of synthesizing iron phosphate using a dual iron source, the solution reaction effect is not good enough and the reaction is incomplete, resulting in a relatively large dead zone area. Therefore, it is necessary to propose a purification method for iron phosphate iron source to solve the above-mentioned problems. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides a method for purifying an iron phosphate source. The purification of the iron phosphate source has the advantages of better economy, and the reaction effect and sufficiency can be reflected during the reaction process. It solves the problem that the existing iron source purification process is not conducive to cost control and the solution reaction effect is not good enough.
[0007] In order to achieve the above-mentioned purification of the iron phosphate source with better economy, and the reaction effect and sufficiency can be reflected in the reaction process, the present invention provides the following technical solution: a purification method of the iron phosphate source, the purification of the iron phosphate source includes the following steps:
[0008] Step 1: first obtain ferrous sulfate heptahydrate and mix with the original aqueous solution, the ratio of ferrous sulfate heptahydrate to the original aqueous solution is 1:1.5, and the two are neutralized to obtain a ferrous clear solution;
[0009] Step 2: Then add ammonia water to the ferrous clear solution, so that the ammonia water and the ferrous clear solution can be easily mixed to obtain a pH value between 2.8-3.3;
[0010] Step 3: Let the mixture of ammonia water and ferrous clear solution stand for half an hour to react, and use reduced iron powder to adjust the pH value to between 3.5-4.5;
[0011] Step 4: Finally, let the solution stand for 20 minutes and then filter it to finally obtain the iron phosphate source.
[0012] Further, the pH of the ferrous solution in step 2 is 2.0, and the pH of the ammonia water is adjusted to 2.89.
[0013] Furthermore, the reduced iron powder in step 3 is adjusted to a pH of 4.1.
[0014] Furthermore, the material composition of the iron phosphate source described in step 4 is: iron: 36.2%, phosphorus: 20.81%, iron-phosphorus ratio: 0.964, potassium: 40ppm, sodium: 25ppm, calcium: 39ppm, magnesium: 24ppm, zinc: 2ppm, chromium: 2ppm, copper: not detected, manganese: 30ppm, D50=2.14um, BET=8.3, tap density: 0.65g / cm3, pH: 2.72.
[0015] Further, the pH of the ferrous solution in step 2 is 2.2, and the pH of the ammonia water is adjusted to 3.2.
[0016] Furthermore, the reduced iron powder in step 3 is adjusted to a pH of 4.0.
[0017] Furthermore, the material composition of the iron phosphate source described in step 4 is: iron: 36.34%, phosphorus: 20.93%, iron-phosphorus ratio: 0.963, potassium: 40ppm, sodium: 16ppm, calcium: 42ppm, magnesium: 25ppm, zinc: 1ppm, chromium: 2ppm, copper: not detected, manganese: 31ppm, D50=2.10um, BET=8.5, tap density: 0.68g / cm3, pH: 2.65.
[0018] Compared with the prior art, the technical solution of this application has the following beneficial effects:
[0019] The method for purifying the ferrous phosphate iron source has been repeatedly verified in the laboratory. After using ammonia water to replace a part of the reduced iron powder, the ferrous sulfate byproduct of titanium dioxide is dissolved, and the pH is adjusted in stages. The ferrous sulfate is dissolved at a ratio of 1:1.5, and the initial pH is between 1.8 and 2.2. The pH of the ferrous solution is first adjusted to 2.8-3.3 using ammonia water, and the reaction is carried out for half an hour without separation. The reduced iron powder is then used to adjust the pH to 3.5-4.5, and the ferrous phosphate iron source is obtained by filtering after reacting for 20 minutes. The reaction residence time is short, the solution reaction time is short, and the reaction effect is good. There is no dead zone in the process of the solution reaction. Compared with the case where all the reduced iron powder is replaced by ammonia water, the phenomenon of liquid and solid being difficult to separate occurs, resulting in the inability to fully filter the ferrous phosphate iron source and wasting a certain amount of raw materials. In comparison, the method has a good cost advantage, so that 50-70 yuan can be saved per ton of ferric phosphate. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a structural flow chart of the iron phosphate iron source purification process of the present invention. DETAILED DESCRIPTION
[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] See also Figure 1 In this embodiment, a method for purifying an iron phosphate source is provided. The purification of the iron phosphate source comprises the following steps:
[0023] Step 1: first obtain ferrous sulfate heptahydrate and mix with the original aqueous solution, the ratio of ferrous sulfate heptahydrate to the original aqueous solution is 1:1.5, and the two are neutralized to obtain a ferrous clear solution;
[0024] Step 2: Then add ammonia water to the ferrous clear solution, so that the ammonia water and the ferrous clear solution can be easily mixed to obtain a pH value between 2.8-3.3;
[0025] Step 3: Let the mixture of ammonia water and ferrous clear solution stand for half an hour to react, and use reduced iron powder to adjust the pH value to between 3.5-4.5;
[0026] Step 4: Finally, let the solution stand for 20 minutes and then filter it to finally obtain the iron phosphate source.
[0027] In the case implementation, the pH of the ferrous solution was adjusted to 2.0, the pH of ammonia water was adjusted to 2.89, and the pH of the reduced iron powder was adjusted to 4.1. The material components of the iron phosphate source finally obtained were: iron: 36.2%, phosphorus: 20.81%, iron-phosphorus ratio: 0.964, potassium: 40ppm, sodium: 25ppm, calcium: 39ppm, magnesium: 24ppm, zinc: 2ppm, chromium: 2ppm, copper: not detected, manganese: 30ppm, D50=2.14um, BET=8.3, tap density: 0.65g / cm3, pH: 2.72.
[0028] In the case implementation, the pH of the ferrous solution was adjusted to 2.2, the pH of ammonia water was adjusted to 3.2, and the pH of the reduced iron powder was adjusted to 4.0. The material components of the iron phosphate source finally obtained were: iron: 36.34%, phosphorus: 20.93%, iron-phosphorus ratio: 0.963, potassium: 40ppm, sodium: 16ppm, calcium: 42ppm, magnesium: 25ppm, zinc: 1ppm, chromium: 2ppm, copper: not detected, manganese: 31ppm, D50=2.10um, BET=8.5, tap density: 0.68g / cm3, pH: 2.65.
[0029] In the case implementation, ammonia water was used to replace a part of the reduced iron powder, and the ferrous sulfate by-product of titanium dioxide was dissolved. The pH was adjusted in stages. The ferrous sulfate was dissolved at a ratio of 1:1.5, and the initial pH was between 1.8-2.2. The pH of the ferrous solution was first adjusted to 2.8-3.3 with ammonia water, and the reaction was continued for half an hour without separation. The reduced iron powder was then used to adjust the pH to 3.5-4.5. After the reaction lasted for 20 minutes, filtration was performed to obtain an iron phosphate source. The reaction residence time was short, the solution reaction time was short, and the reaction effect was good. There would be no dead zone during the solution reaction.
[0030] In the case implementation, compared with using ammonia water to replace the reduced iron powder, the liquid and solid are difficult to separate, resulting in the inability to fully filter the iron phosphate source, wasting a certain amount of raw materials, and because the solution reacts more completely during the reaction process, the quality of the output iron phosphate source after complete filtration is basically the same as that of the whole iron powder, so that the cost raw materials can be better reduced and retained. In comparison, the present invention has a better cost advantage, which can save 50-70 yuan in cost benefits per ton of iron phosphate, greatly saving cost raw materials.
[0031] In summary, the purification method of the iron phosphate iron source, the present invention has been repeatedly verified in the laboratory, by using ammonia water to replace a part of the reduced iron powder, dissolving the titanium dioxide byproduct ferrous sulfate, and adjusting the pH in stages, by dissolving the ferrous sulfate according to a ratio of 1:1.5, the initial pH is between 1.8-2.2, first using ammonia water to adjust the pH of the ferrous solution to 2.8-3.3, reacting for half an hour without separation, and then using reduced iron powder to adjust the pH to 3.5-4.5, reacting for 20 minutes, filtering and other operations to obtain the iron phosphate iron source, the reaction residence time is short, the solution reaction time is short and the reaction effect is better, and there will be no dead zone unreacted during the solution reaction; compared with the use of ammonia water to replace the reduced iron powder, the phenomenon of liquid and solid separation is difficult, resulting in the iron phosphate iron source cannot be fully filtered, wasting a certain amount of raw materials, by comparison, the present invention has a good cost advantage, so that each ton of iron phosphate can save 50-70 yuan.
[0032] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0033] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for purifying an iron phosphate source, characterized in that: The purification of the iron phosphate source includes the following steps: Step 1: first obtain ferrous sulfate heptahydrate and mix with the original aqueous solution, the ratio of ferrous sulfate heptahydrate to the original aqueous solution is 1:1.5, and the two are neutralized to obtain a ferrous clear solution; Step 2: Then add ammonia water to the ferrous clear solution, so that the ammonia water and the ferrous clear solution can be easily mixed to obtain a pH value between 2.8-3.3; Step 3: Let the mixture of ammonia water and ferrous clear solution stand for half an hour to react, and use reduced iron powder to adjust the pH value to between 3.5-4.5; Step 4: Finally, let the solution stand for 20 minutes and then filter it to finally obtain the iron phosphate source.
2. The method for purifying an iron phosphate source according to claim 1, characterized in that: The pH of the ferrous solution in step 2 is 2.0, and the pH of the ammonia water is adjusted to 2.
89.
3. The method for purifying an iron phosphate source according to claim 1, characterized in that: The reduced iron powder in step 3 is adjusted to a pH of 4.
1.
4. A method for purifying an iron phosphate source according to claims 2 and 3, characterized in that: The material composition of the iron phosphate source described in step 4 is as follows: iron: 36.2%, phosphorus: 20.81%, iron-phosphorus ratio: 0.964, potassium: 40ppm, sodium: 25ppm, calcium: 39ppm, magnesium: 24ppm, zinc: 2ppm, chromium: 2ppm, copper: not detected, manganese: 30ppm, D50=2.14um, BET=8.3, tap density: 0.65g / cm3, pH: 2.
72.
5. The method for purifying an iron phosphate source according to claim 1, characterized in that: The pH of the ferrous solution in step 2 is 2.2, and the pH of the ammonia water is adjusted to 3.
2.
6. The method for purifying an iron phosphate source according to claim 1, characterized in that: The reduced iron powder in step 3 is adjusted to a pH of 4.
0.
7. A method for purifying an iron phosphate source according to claims 5 and 6, characterized in that: The material composition of the iron phosphate source described in step 4 is as follows: iron: 36.34%, phosphorus: 20.93%, iron-phosphorus ratio: 0.963, potassium: 40ppm, sodium: 16ppm, calcium: 42ppm, magnesium: 25ppm, zinc: 1ppm, chromium: 2ppm, copper: not detected, manganese: 31ppm, D50=2.10um, BET=8.5, tap density: 0.68g / cm3, pH: 2.65.
Citation Information
Patent Citations
Refining method of titanium dioxide by-product ferrous sulphate
CN103145197A
Impurity removal method for titanium dioxide byproduct ferrous sulfate
CN117534125A
Method for preparing ferrous sulfate from titanium dioxide byproduct ferrous sulfate
CN117756189A
Method for preparing iron phosphate and use thereof
WO2022116702A1