Solvothermal synthesis method of thin-film solar cell material cesium-lead-halogen nanocrystal
Through solvent thermal synthesis method and n-octylphosphonic acid ligand modification, the stability of cesium lead-halide nanocrystals is improved, the structural instability problem in humid environments is solved, and its application potential in solar cells is realized. Simple process, low cost and environmentally friendly.
Patent Information
- Application Number
- CN202410907249.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
AI Technical Summary
All-inorganic cesium lead-halide nanocrystals have poor crystal structure stability in humid environments, which hinders its widespread application in solar cells.
The cesium lead-halide nanocrystals were prepared by solvent thermal synthesis method. The corresponding compound was weighed through the stoichiometric ratio of the chemical formula CsPbIxBr3-x, and the solvent and co-solvent were added. After stirring and dissolving, the reaction was carried out at 120°C to 180°C, and it was cooled naturally and left to stand. The stratification was performed and centrifuged to obtain stable nanocrystals, and n-octylphosphonic acid was used as a ligand to improve the stability of the nanocrystals.
It realizes high stability of cesium lead-halide nanocrystals, can be stored in deionized water and in air with high humidity for a long time, reduces energy consumption and environmental pollution, and is suitable for commercial production, and the product has a small average particle size and narrow Particle size distribution and good dispersion.
Smart Images

Figure CN118877929A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for synthesizing a thin-film solar cell material. Background Art
[0002] All-inorganic cesium lead halide CsPbI x Br 3-x (0≤x≤3) nanocrystals can be used as light-absorbing materials for perovskite solar cells and light-emitting diodes due to their excellent optical properties, adjustable band gap, high carrier mobility and photoluminescence quantum yield, and narrow half-peak width of luminescence. Cesium lead halide nanocrystals are ABX with perovskite structure type. 3 The cesium lead halide nanocrystals are a type of compound, and the crystal structure is characterized by the coexistence of ions with greatly different radii, and the efficiency of absorbing light is higher than that of silicon. The equipment required to integrate cesium lead halide nanocrystals into solar cells is relatively simple. The nanocrystals can be dissolved in a solvent and sprayed directly onto the substrate. Therefore, they are very suitable as the active layer of solar cells to absorb light. The biggest advantage of all-inorganic cesium lead halide nanocrystals is that, on the one hand, the photoelectric properties of perovskite materials can be regulated by replacing halogen ions, and by changing the ratio of different halogen ions, the band gap of nanocrystals can be adjusted, reducing the loss of holes at the interface, thereby improving the photoelectric conversion efficiency of perovskite solar cells; on the other hand, their high temperature stability is better than that of organic-inorganic hybrid lead halide nanocrystals. Among them, CsPbI 3 The bandgap width of CsPbI is the smallest, the wavelength range of light that can be absorbed is wider, and the efficiency of solar cells is higher. x Br 3-x (0≤x≤3) nanocrystals in a humid environment, or even in air, still face great obstacles to their application. Therefore, surface modification technology is used to improve the x Br 3-x (0≤x≤3)The stability of nanocrystals has important theoretical value and engineering significance. Summary of the invention
[0003] The present invention aims to solve the problem of poor crystal structure stability of existing cesium lead halide nanocrystals as thin-film solar cell materials, and further provides a solvent thermal synthesis method of cesium lead halide nanocrystals as thin-film solar cell materials.
[0004] A solvent thermal synthesis method of cesium lead halide nanocrystals as a thin film solar cell material is carried out according to the following steps:
[0005] 1. According to the chemical formula CsPbI x Br 3-x A cesium source compound, a lead source compound, an iodine source compound and a bromine source compound are weighed in a stoichiometric ratio to obtain a raw material;
[0006] The chemical formula is CsPbI x Br 3-x 0≤x≤3;
[0007] 2. Add the raw materials into the solvent, then add n-octylphosphonic acid and a co-solvent, and finally stir and dissolve to obtain a mixed solution;
[0008] 3. reacting the mixed solution at a temperature of 120° C. to 180° C. for 20 min to 200 min, and finally naturally cooling to room temperature to obtain a reaction system;
[0009] 4. The reaction system is allowed to stand for stratification, and after removing the supernatant, n-hexane is added for centrifugal washing, and finally dried, thereby completing the solvothermal synthesis method of cesium lead halide nanocrystals as a thin-film solar cell material.
[0010] The beneficial effects of the present invention are:
[0011] The preparation method of the present invention has the characteristics of low raw material cost, simple process, low reaction temperature, short reaction time, etc., can reduce energy consumption, has little environmental pollution, and is suitable for commercial production. The final product of the present invention is a single-phase CsPbI x Br 3-x (0≤x≤3) nanocrystals, small average particle size, narrow particle size distribution, good dispersibility, and controllable size. x Br 3-x Nanocrystals (CsPbI x Br 3-x NCs) have a strong bonding effect. After the -OH in the phosphonic acid is deprotonated, it binds to Pb 2+ At the same time, another -OH is combined with -P=O through hydrogen bonding, which significantly improves the affinity of phosphonic acid with CsPbBr 3 The bonding strength of NCs surface improves the CsPbBr 3 The stability of NCs can be stably stored in deionized water and in air at 25°C and 40% humidity for 2 days and 30 days, respectively.
[0012] Instruction Manual
[0013] Figure 1 XRD spectra of cesium lead halide nanocrystals of thin-film solar cell materials prepared in Examples 1 to 3;
[0014] Figure 2 The thin-film solar cell material cesium lead halide nanocrystal (CsPbI 3 ) XRD spectra after being stored in deionized water at room temperature for different time periods;
[0015] Figure 3The thin-film solar cell material cesium lead halide nanocrystal (CsPbI 3 ) XRD spectra after being stored in air (temperature 25°C, humidity 40%) for different time periods;
[0016] Figure 4 The thin-film solar cell material cesium lead halide nanocrystal (CsPbI 3 )’s full XPS spectrum;
[0017] Figure 5 The thin-film solar cell material cesium lead halide nanocrystal (CsPbI 3 )
[0018] Figure 6 The thin-film solar cell material cesium lead halide nanocrystal (CsPbI 3 ) Absorption spectra after being stored in deionized water at room temperature for different time periods. DETAILED DESCRIPTION
[0019] Specific implementation method 1: This implementation method is a solvent thermal synthesis method of cesium lead halide nanocrystals of thin film solar cell materials, which is carried out according to the following steps:
[0020] 1. According to the chemical formula CsPbI x Br 3-x A cesium source compound, a lead source compound, an iodine source compound and a bromine source compound are weighed in a stoichiometric ratio to obtain a raw material;
[0021] The chemical formula is CsPbI x Br 3-x 0≤x≤3;
[0022] 2. Add the raw materials into the solvent, then add n-octylphosphonic acid and a co-solvent, and finally stir and dissolve to obtain a mixed solution;
[0023] 3. reacting the mixed solution at a temperature of 120° C. to 180° C. for 20 min to 200 min, and finally naturally cooling to room temperature to obtain a reaction system;
[0024] 4. The reaction system is allowed to stand for stratification, and after removing the supernatant, n-hexane is added for centrifugal washing, and finally dried, thereby completing the solvothermal synthesis method of cesium lead halide nanocrystals as a thin-film solar cell material.
[0025] The beneficial effects of this embodiment are:
[0026] The preparation method of this embodiment has the characteristics of low raw material cost, simple process, low reaction temperature, short reaction time, etc., which can reduce energy consumption, cause little environmental pollution, and is suitable for commercial production. The final product of this embodiment is a single-phase CsPbI x Br 3-x (0≤x≤3) nanocrystals, small average particle size, narrow particle size distribution, good dispersibility, and controllable size. x Br 3-x Nanocrystals (CsPbI x Br 3-x NCs) have a strong bonding effect. After the -OH in the phosphonic acid is deprotonated, it binds to Pb 2+ At the same time, another -OH is combined with -P=O through hydrogen bonding, which significantly improves the affinity of phosphonic acid with CsPbBr 3 The bonding strength of NCs surface improves the CsPbBr 3 The stability of NCs can be stably stored in deionized water and in air at 25°C and 40% humidity for 2 days and 30 days, respectively.
[0027] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that the cesium source compound in step 1 is cesium chloride, cesium nitrate, cesium carbonate, cesium acetate or cesium sulfate. The rest is the same as specific embodiment 1.
[0028] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the lead source compound in step 1 is lead iodide, lead bromide or lead acetate. The rest is the same as specific implementation method 1 or 2.
[0029] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the iodine source compound in step 1 is lead iodide or methylamine iodine. The rest is the same as specific embodiments 1 to 3.
[0030] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the bromine source compound in step 1 is lead bromide, cesium bromide or iodine bromide. Other aspects are the same as specific embodiments 1 to 4.
[0031] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that: the solvent in step 2 is octadecene; the cosolvent in step 2 is tri-n-octylphosphine oxide and tri-n-octylphosphine, or a mixture of two thereof. The rest is the same as specific embodiments 1 to 5.
[0032] Specific embodiment 7: This embodiment differs from Specific embodiments 1 to 6 in that the volume ratio of the amount of the raw material and the solvent in step 2 is 1 mmol: (20-50) mL. The rest is the same as Specific embodiments 1 to 6.
[0033] Specific embodiment 8: This embodiment differs from Specific embodiments 1 to 7 in that the mass ratio of the amount of the raw material in step 2 to n-octylphosphonic acid is 1 mmol: (70-120) mg. The rest is the same as Specific embodiments 1 to 7.
[0034] Specific embodiment 9: This embodiment differs from Specific embodiments 1 to 8 in that: the mass ratio of the amount of the raw material in step 2 to the co-solvent is 1 mmol: (1 to 5) g; or the volume ratio of the amount of the raw material in step 2 to the co-solvent is 1 mmol: (5 to 10) mL. Others are the same as Specific embodiments 1 to 8.
[0035] Specific embodiment 10: This embodiment differs from Specific embodiments 1 to 9 in that the stirring and dissolving in step 2 is carried out at a temperature of 25° C. to 60° C. for 30 min to 300 min. The rest is the same as Specific embodiments 1 to 9.
[0036] The following examples are used to verify the beneficial effects of the present invention:
[0037] Embodiment 1:
[0038] A solvent thermal synthesis method of cesium lead halide nanocrystals as a thin film solar cell material is carried out according to the following steps:
[0039] 1. According to the chemical formula CsPbI x Br 3-x Cesium acetate and lead bromide are weighed in a stoichiometric ratio to obtain a raw material;
[0040] The chemical formula is CsPbI x Br 3-x x=0;
[0041] 2. Add the raw materials into octadecene (ODE), then add n-octylphosphonic acid (OPA) and tri-n-octylphosphine oxide (TOPO), and finally stir for 30 minutes at a temperature of 45°C to obtain a mixed solution;
[0042] The volume ratio of the amount of the raw material to octadecene is 1 mmol:50 mL; the mass ratio of the amount of the raw material to n-octylphosphonic acid is 1 mmol:110 mg; the mass ratio of the amount of the raw material to tri-n-octylphosphine oxide is 1 mmol:4 g;
[0043] 3. reacting the mixed solution at 160° C. for 30 min, and finally cooling naturally to room temperature to obtain a reaction system;
[0044] 4. The reaction system was allowed to stand for stratification, and after removing the supernatant, n-hexane was added for centrifugal washing, and finally dried to obtain cesium lead halide nanocrystals, i.e., CsPbBr, a thin-film solar cell material. 3 , that is, the solvothermal synthesis method of cesium lead halide nanocrystals as thin-film solar cell materials is completed.
[0045] Example 2: This example is different from Example 1 in that: in step 1, according to the chemical formula CsPbI x Br 3-x Cesium acetate, lead iodide and lead bromide are weighed in a stoichiometric ratio to obtain a raw material; the chemical formula is CsPbI x Br 3-x In step 4, cesium lead halide nanocrystals, i.e., CsPbIBr, are obtained as thin-film solar cell materials. 2 The rest is the same as that of the first embodiment.
[0046] Example 3: This example is different from Example 1 in that: in step 1, according to the chemical formula CsPbI x Br 3-x Cesium acetate, lead iodide and lead bromide are weighed in a stoichiometric ratio to obtain a raw material; the chemical formula is CsPbI x Br 3-x Where x=2; Step 4: Get cesium lead halide nanocrystals, i.e. CsPbI 2 Br. The rest is the same as in Example 1.
[0047] Embodiment 4:
[0048] A solvent thermal synthesis method of cesium lead halide nanocrystals as a thin film solar cell material is carried out according to the following steps:
[0049] 1. According to the chemical formula CsPbI x Br 3-x Cesium carbonate and lead iodide are weighed in a stoichiometric ratio to obtain a raw material;
[0050] The chemical formula is CsPbI x Br 3-x x=3;
[0051] 2. Add the raw materials to octadecene, then add n-octylphosphonic acid (OPA), tri-n-octylphosphine oxide (TOPO) and tri-n-octylphosphine (TOP), and finally stir for 60 minutes at a temperature of 40° C. to obtain a mixed solution;
[0052] The volume ratio of the amount of the raw material to octadecene is 1 mmol:36 mL; the mass ratio of the amount of the raw material to n-octylphosphonic acid is 1 mmol:95 mg; the mass ratio of the amount of the raw material to tri-n-octylphosphine oxide is 1 mmol:1.2 g; the volume ratio of the amount of the raw material to tri-n-octylphosphine is 1 mmol:5 mL;
[0053] 3. reacting the mixed solution at 160° C. for 20 min, and finally cooling naturally to room temperature to obtain a reaction system;
[0054] 4. The reaction system was allowed to stand for stratification, and after removing the supernatant, n-hexane was added for centrifugal washing, and finally dried to obtain cesium lead halide nanocrystals, i.e. CsPbI thin film solar cell materials. 3 , that is, the solvothermal synthesis method of cesium lead halide nanocrystals as thin-film solar cell materials is completed.
[0055] Figure 1 The XRD spectra of the cesium lead halide nanocrystals of thin-film solar cell materials prepared in Examples 1 to 3 are shown in the figure. As can be seen from the figure, the diffraction peaks of the obtained materials are relatively high and sharp, and the characteristic peaks are 2θ=15.1°, 21.4°, 30.3° and 35.2°, respectively corresponding to the (100), (110), (200) and (210) crystal planes; no obvious impurity peaks exist. This shows that the method can be used to prepare pure phase cesium lead halide nanocrystals with good crystallinity.
[0056] Figure 2 The thin-film solar cell material cesium lead halide nanocrystal (CsPbI 3 ) after being stored in deionized water at room temperature for different time periods; As can be seen from the figure, the CsPbI modified with n-octylphosphonic acid (OPA) ligand 3 The nanocrystals can be stored stably in water for two days. 3 As the nanocrystals are stored in water for a longer time, the diffraction peaks of octylphosphonic acid near 11° gradually increase, while the diffraction peaks of CsPbI near 25-30° and 37° gradually increase. 3 The diffraction peak intensity of the nanocrystals gradually decreased, indicating that with the extension of time, the OPA ligand gradually changed from CsPbI 3 Nanocrystal surface detachment, CsPbI 3 The nanocrystal structure is gradually destroyed. At the same time, the PbI 2 The diffraction peaks show that with the extension of time, PbI 2 The diffraction peak intensity of CsPbI 3 The nanocrystal crystal structure decomposes and gradually generates PbI 2 , but CsPbI 3After the nanocrystals were placed in water for 3 days, weak CsPbI can still be detected in the product. 3 The diffraction peaks indicate that CsPbI 3 After being placed in water for 3 days, most of the nanocrystals decomposed, but some CsPbI 3 Mutually.
[0057] Figure 3 The thin-film solar cell material cesium lead halide nanocrystal (CsPbI 3 ) after being stored in air (temperature 25°C, humidity 40%) for different time periods; As can be seen from the figure, OPA ligand-modified CsPbI 3 After the nanocrystals were stored in air for 30 days, the crystal structure remained unchanged and the sharp CsPbI 3 Phase diffraction peak, no obvious PbI 2 phase formation, which indicates that OPA significantly improves the 3 The crystal structure stability of nanocrystals inhibits the 3 The crystal structure of the phase decomposition.
[0058] Figure 4 The thin-film solar cell material cesium lead halide nanocrystal (CsPbI 3 ) full XPS spectrum; As can be seen from the figure, in CsPbI 3 Obvious phosphorus was detected in the nanocrystals, and the peak position of P2p in the figure corresponds to the P=O bond, which proves that the OPA ligand is 3 The nanocrystal surface was successfully adsorbed.
[0059] Figure 5 The thin-film solar cell material cesium lead halide nanocrystal (CsPbI 3 ) SEM photo; As can be seen from the figure, OPA ligand-modified CsPbI 3 The nanocrystals are flaky, with a small average particle size, narrow particle size distribution, and good dispersibility. Since the OPA ligands are well combined with the nanocrystals, and the OPA ligands can also be connected by hydrogen bonds, the CsPbI 3 The growth of nanocrystals in the adsorption direction makes CsPbI 3 The nanocrystals exhibit a flake-like morphology.
[0060] Figure 6 The thin-film solar cell material cesium lead halide nanocrystal (CsPbI 3) Absorption spectra of CsPbI after being stored in deionized water at room temperature for different time periods. As can be seen from the figure, there is a weak absorption behavior in the wavelength range of 800nm to 1200nm, which is mainly due to the slight decrease in the quantum confinement effect caused by the size of the nanocrystals synthesized by solvent thermal synthesis. There is an obvious optical absorption peak near 430nm. As the storage time in water increases, the absorption peak position does not change significantly, but CsPbI 3 The absorption coefficient of nanocrystals decreases as a whole, indicating that as the storage time in water increases, CsPbI 3 Nanocrystals decompose and their optical absorption capacity decreases. CsPbI 3 The absorption coefficient of the nanocrystals decreased by about 50% after being stored in water for 3 days, but they still had a certain optical absorption capacity.
Claims
1. A solvent thermal synthesis method for cesium lead halide nanocrystals as thin film solar cell materials, characterized in that It is carried out in the following steps:
1. According to the chemical formula CsPbI x Br 3-x A cesium source compound, a lead source compound, an iodine source compound, and a bromine source compound are weighed in a stoichiometric ratio to obtain a raw material; The chemical formula CsPbI x Br 3-x 0≤x≤3; 2. Add the raw materials into the solvent, then add n-octylphosphonic acid and cosolvent, and finally stir and dissolve to obtain a mixed solution; 3. reacting the mixed solution at a temperature of 120° C. to 180° C. for 20 min to 200 min, and finally naturally cooling to room temperature to obtain a reaction system; 4. The reaction system is allowed to stand for stratification, and after removing the supernatant, n-hexane is added for centrifugal washing, and finally dried, thereby completing the solvent thermal synthesis method of cesium lead halide nanocrystals as a thin film solar cell material.
2. The solvent thermal synthesis method of cesium lead halide nanocrystals as a thin film solar cell material according to claim 1, characterized in that The cesium source compound in step 1 is cesium chloride, cesium nitrate, cesium carbonate, cesium acetate or cesium sulfate.
3. The solvent thermal synthesis method of cesium lead halide nanocrystals as a thin film solar cell material according to claim 1, characterized in that The lead source compound described in step 1 is lead iodide, lead bromide or lead acetate.
4. The solvent thermal synthesis method of cesium lead halide nanocrystals as a thin film solar cell material according to claim 1, characterized in that The iodine source compound described in step 1 is lead iodide or methylamine iodide.
5. The solvothermal synthesis method of cesium lead halide nanocrystals as a thin film solar cell material according to claim 1, characterized in that The bromine source compound in step 1 is lead bromide, cesium bromide or iodine bromide.
6. The solvothermal synthesis method of cesium lead halide nanocrystals as a thin film solar cell material according to claim 1, characterized in that The solvent in step 2 is octadecene; the cosolvent in step 2 is tri-n-octylphosphine oxide and tri-n-octylphosphine, or a mixture of both.
7. The solvothermal synthesis method of cesium lead halide nanocrystals as a thin film solar cell material according to claim 1, characterized in that The volume ratio of the amount of the raw material described in step 2 to the solvent is 1 mmol: (20-50) mL.
8. The solvothermal synthesis method of cesium lead halide nanocrystals as a thin film solar cell material according to claim 1, characterized in that The mass ratio of the amount of the raw material described in step 2 to n-octylphosphonic acid is 1 mmol: (70-120) mg.
9. The solvothermal synthesis method of cesium lead halide nanocrystals as a thin film solar cell material according to claim 1, characterized in that The mass ratio of the amount of the raw material described in step 2 to the co-solvent is 1 mmol: (1 to 5) g; or the volume ratio of the amount of the raw material described in step 2 to the co-solvent is 1 mmol: (5 to 10) mL.
10. The solvothermal synthesis method of cesium lead halide nanocrystals as a thin film solar cell material according to claim 1, characterized in that The stirring and dissolving in step 2 is specifically carried out at a temperature of 25° C. to 60° C. and stirring for 30 min to 300 min.