WO3 / MGO nano composite material as well as preparation method and application thereof

By growing nanorod-shaped WO3 on the surface of the ceramic plate and hydrothermal reaction with edge graphene oxide to form WO3/MGO nanocomposite, the high power consumption and poor selectivity of the sensor when detecting toxic and harmful gases are solved, and the three-B High selective detection of amine and formaldehyde gases and adapting to different gases through temperature adjustment, improving the sensitivity and service life of the sensor.

CN118877943APending Publication Date: 2024-11-01SHANDONG JINLIT NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410809426.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing sensors have high power consumption and poor selectivity when detecting toxic and harmful gases, which are prone to false alarms and accidental contacts, and have a single function and need to be replaced frequently, which affects the accuracy and safety of detection.

Method used

WO3/MGO nanocomposite material is used as the sensing layer material, and nanorod-shaped WO3 is grown on the surface of the ceramic plate by controlling the pH value and growth time, and hydrothermal reaction with edge graphene oxide to form WO3/MGO nanocomposite material and enlargement The contact area of ​​gas molecules and electron transport efficiency simplifies the preparation process and improves the sensitivity of the sensor.

Benefits of technology

High selective detection of triethylamine and formaldehyde gases is achieved, reducing the frequency of sensor replacement, and adapting to different gas detection by adjusting the working temperature, improving the service life and application convenience of the sensor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118877943A_ABST
    Figure CN118877943A_ABST
Patent Text Reader

Abstract

The invention provides a WO3 / MGO nano composite material and a preparation method and application thereof, and relates to the field of nano composite materials, and the method comprises the following steps: taking Na2WO4. 2H2O to prepare a solution A; slowly dropwise adding concentrated hydrochloric acid into the solution A, and diluting to obtain a solution B; adding citric acid dihydrate into the solution B to adjust the pH value, and adding water to dilute to obtain a solution C; adding sodium chloride into the solution C to obtain a solution D; placing a base material in a reaction container, placing the solution D in the reaction container, and controlling the temperature and time in the reaction container to enable WO3 to grow on the surface of the base material; the preparation method comprises the following steps: dissolving edge graphene oxide MGO subjected to high-temperature treatment in a solvent to prepare an MGO dispersion solution; carrying out hydrothermal reaction on the MGO dispersion solution and a base material to obtain a WO3 / MGO nano composite material; the obtained nano composite material can be used as a sensing layer of the gas sensor; according to the invention, the subsequent coating step is avoided, the process is simple, large-scale batch production is facilitated, and the material can realize selective detection of two gases of triethylamine and formaldehyde.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nanocomposite materials, and in particular to a WO3 / MGO nanocomposite material used in the field of toxic and harmful gas detection, and a preparation method and application thereof. Background Art

[0002] With the rapid development of science and technology and the gradual advancement of industrialization and urbanization, air pollution is becoming increasingly serious. According to surveys, the degree of indoor air pollution is much greater than that of outdoor air, especially in places where industrial parks are crowded and the environment is relatively sealed. As time goes by, many harmful gases are produced in the air, which seriously endangers human health. Indoor toxic and harmful gases are roughly formaldehyde, ammonia, etc. Various indoor air pollutants will cause varying degrees of damage to the human body. Therefore, it is particularly important to detect air and conduct early warning research, which is directly related to people's work, life, health, and the stable development of society.

[0003] At present, most of the sensors on the market use ZnO and SnO2 as the core materials to detect toxic and harmful gases in the air, but there are some problems such as high power consumption, poor selectivity, and easy false alarms. It is difficult for traditional metal oxides to detect toxic and harmful gases. In addition, after a period of use, the accuracy of the sensor will decline to a certain extent. Once the accuracy of the detection cannot be maintained, serious accidents that damage people's health may occur; the existing solution is to replace the sensor regularly, but frequent replacement consumes too much. Finally, the functions of existing sensors are too fixed, and the detection target of each sensor is too single. The existing research plan is to select different types of sensors according to the different gases to be detected, which is inconvenient in actual operation. Summary of the invention

[0004] In view of the above problems existing in the prior art, the present invention provides a WO3 / MGO nanocomposite material and a preparation method and application thereof.

[0005] The technical solution of the present invention to solve the above technical problems is as follows:

[0006] In a first aspect, the present invention provides a WO3 / MGO nanocomposite material and a preparation method thereof, wherein the preparation method comprises the following steps:

[0007] Dissolve Na2WO4·2H2O in water to obtain solution A; slowly drop concentrated hydrochloric acid into solution A, stir after adding, and dilute with pure water to obtain solution B; add citric acid dihydrate to solution B until the pH of the solution reaches 2.6, stir, and dilute with water to obtain solution C; add sodium chloride to solution C to obtain solution D;

[0008] Place the substrate in a reaction container, place solution D in the reaction container, control the temperature and time in the reaction container to grow WO3 on the surface of the substrate; take out the substrate, wash it, and dry it for later use; in this step, nanorod-shaped WO3 is obtained by controlling the pH value, and the size of the WO3 nanorod is controlled by controlling the growth time, and the size of the WO3 prepared by this method is uniform and does not need to be subjected to subsequent high-temperature calcination treatment; MGO has a large specific surface area and considerable electronic conductivity, which can not only increase the contact area of ​​the material with harmful gas molecules, but also improve the sensitivity of the sensor by improving the electronic transmission efficiency of WO3;

[0009] The edge graphene oxide MGO treated at high temperature is dissolved in a solvent to prepare an MGO dispersion solution; the MGO dispersion solution and the substrate are transferred to a reaction container, the temperature is controlled to perform a hydrothermal reaction, and after cooling to room temperature, the substrate is taken out, and after washing and drying, a composite material based on WO3 grown with MGO located on the surface of the substrate, namely, a WO3 / MGO nanocomposite material, is obtained.

[0010] Furthermore, the raw material edge graphene oxide, namely MGO, can be edge graphene oxide prepared by the Hummers method, which is suitable for industrial mass production.

[0011] Furthermore, the substrate is a ceramic plate.

[0012] Furthermore, the temperature of the high temperature treatment is 900-2500°C.

[0013] Furthermore, the temperature in the reaction container is controlled at 100° C. to allow WO 3 to grow on the surface of the substrate.

[0014] Furthermore, the solvent is ethanol.

[0015] Furthermore, the temperature of the hydrothermal reaction is 200°C.

[0016] In a second aspect, the present invention provides an application of the above-mentioned WO3 / MGO nanocomposite material, characterized in that it is used for preparing a gas sensor, wherein the WO3 / MGO nanocomposite material is used as a gas sensitive material and as a sensing layer material of the gas sensor.

[0017] Furthermore, the gas sensor is used to detect triethylamine and formaldehyde gases.

[0018] Furthermore, when the operating temperature is 180°C, the gas sensor is used to detect triethylamine gas; when the operating temperature is 300°C, the gas sensor is used to detect formaldehyde gas.

[0019] The beneficial effects of the present invention are:

[0020] 1. The present invention provides a method for preparing a WO3 nanocomposite material grown on the surface of edge graphene oxide, wherein the nanorod-shaped WO3 is directly grown on the surface of a substrate by controlling the pH of the system, and then hydrothermally reacted with MGO to obtain a composite material based on WO3 grown with MGO on the surface of the substrate, i.e., a WO3 / MGO nanocomposite material. The method grows the composite material directly on the ceramic plate substrate, avoids the subsequent coating step, has a simple process, and is conducive to large-scale batch production.

[0021] 2. The WO3 / MGO nanocomposite material prepared by the present invention utilizes the large specific surface area of ​​edge graphene oxide, and the composite with WO3 can significantly increase the specific surface area of ​​WO3, thereby enhancing the contact between the composite material and the gas molecules to be measured and thus improving the performance of the sensor; and because of the presence of its chemically active groups, it can help fix the nano WO3, thereby playing a protective role on it, preventing the nanorods from agglomerating and unevenly dispersing, which affects the service life of the sensing material.

[0022] 3. The WO3 / MGO nanocomposite prepared by the present invention is applied to toxic and harmful gas sensors, which can specifically realize the selective detection of triethylamine and formaldehyde gases, reducing the problem of replacing sensors when detecting different gases; in gas testing, high-selective detection of triethylamine and formaldehyde can be realized by only changing the current working temperature, which greatly enriches the application field, and different working temperatures can be set according to the type of detected gas. The obtained ceramic substrate carrying the WO3 / MGO nanocomposite can be directly used as a gas-sensitive ceramic, which greatly simplifies the preparation process of the gas sensor. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 1 is a curve diagram of the detection sensitivity of the sensor prepared in Example 1 and Comparative Example 1 to triethylamine and formaldehyde gas respectively;

[0024] Figure 2 1 is a selectivity test diagram of the sensor prepared in the embodiment for triethylamine and formaldehyde gas at 180° C. and 300° C. respectively;

[0025] Figure 3 is a SEM image of the WO3 / MGO nanocomposite material prepared in Example;

[0026] Figure 4 (A) is a SEM image of the composite material prepared in Comparative Example 2;

[0027] Figure 4 (B) is a SEM image of the composite material prepared in Comparative Example 3;

[0028] Figure 5 is a schematic cross-sectional structural diagram of a flat ceramic plate prepared in the embodiment as a gas-sensitive ceramic;

[0029] Figure 6 It is the structure and measurement circuit of the existing MQN gas sensor;

[0030] In the figure: 1. Flat ceramic, 2. Comb-shaped heating belt. DETAILED DESCRIPTION

[0031] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0032] The main raw materials involved in the following examples are as follows:

[0033] Edge oxidized graphene: Edge oxidized graphene prepared by conventional Hummers, the specific process is: put 10g of graphite (Aladdin Biochemical Technology Co., Ltd., P196402) into 500mL concentrated sulfuric acid and stir for 120min. After stirring is completed, place the container on the laboratory bench to cool to room temperature, slowly add 5g of sodium nitrate to the above mixed solution, and stir for 15min. After repeatedly placing the container in the outside to cool to room temperature, add 50g of potassium ferrate (in the process of adding potassium ferrate, add a small amount multiple times, keep stirring quickly, and control the temperature to be below 15°C throughout the process to prevent excessive addition and system temperature from causing liquid splashing or explosion), and stir for 240min. After the above reaction is completed, add 2000mL of deionized water to dilute (add water evenly during the process of adding water, keep stirring quickly, prevent the system temperature from rising sharply due to dilution and reducing MGO, and freeze 2000mL of water into ice cubes, and then move the feed liquid into the ice cubes for dilution), the experimental reaction is violent. After the temperature drops to room temperature, add excess H2O2 (add hydrogen peroxide in small amounts and multiple times, and stir the liquid quickly during the addition process to prevent the large amount of bubbles generated by the first excessive addition from being unable to dissipate and affecting the subsequent addition of hydrogen peroxide), generate a large number of bubbles, and after the reaction is completed, MGO powder is obtained. Excess impurities are washed off with hydrochloric acid, deionized water and ethanol to obtain MGO powder.

[0034] Na2WO4·2H2O: Aladdin Biochemical Technology Co., Ltd., S305386;

[0035] Citric acid monohydrate: Aladdin Biochemical Technology Co., Ltd., C112632.

[0036] Example

[0037] The preparation method of the WO3 / MGO nanocomposite material of this embodiment is as follows:

[0038] S1. High-temperature treatment of edge graphene oxide, i.e., MGO powder: The MGO powder is placed in a tube furnace for high-temperature treatment, argon gas is introduced, and the temperature is raised from room temperature to 900°C at 4°C / min. After reaching 900°C, the temperature is kept at 900°C for 30 minutes, and black MGO powder is obtained after the temperature is cooled.

[0039] S2. Take 3.72g Na2WO4·2H2O and dissolve it in 10mL distilled water, stir for 30min, and obtain solution A; take 5mL 12M concentrated hydrochloric acid and slowly add it dropwise to the above solution, stir for 30min after the addition is complete, then add pure water to dilute to 50ml, and obtain solution B; add citric acid dihydrate to solution B until the pH of the solution reaches 2.6, stir for 30min, then add deionized water to dilute to 40mL to obtain solution C. Add 1.5g sodium chloride to solution C, stir for 120min, and obtain solution D.

[0040] S3, take a flat ceramic plate as a substrate, clean it with ultrasound, dry it, and place it at the bottom of a reactor, place solution D in the reaction vessel, and after heating at 100°C for 12 hours, WO3 grows on the surface of the ceramic plate; take out the ceramic plate, clean it, and dry it for later use;

[0041] S4. Dissolve 10 g of high-temperature treated MGO in 45 mL of ethanol and stir evenly to prepare an MGO ethanol dispersion solution; transfer the MGO ethanol dispersion solution and the ceramic plate to a reactor, perform a hydrothermal reaction at 200° C. for 5 h, cool to room temperature, take out the ceramic plate, wash it with pure water and anhydrous ethanol, and dry it to obtain a composite material based on WO3 grown with MGO on the surface of the ceramic plate, namely, a WO3 / MGO nanocomposite material.

[0042] Comparative Example 1

[0043] The preparation method of this comparative example is the same as S2 and S3 of the embodiment, except that it does not include steps S1 and S4 of the embodiment. Specifically:

[0044] S1. Dissolve 3.72g Na2WO4·2H2O in 10mL distilled water and stir for 30min to obtain solution A; slowly drop 5mL 12M concentrated hydrochloric acid into the above solution, stir for 30min after addition, then add pure water to dilute to 50ml to obtain solution B; add citric acid dihydrate to solution B until the pH of the solution reaches 2.6, stir for 30min, then add deionized water to dilute to 40mL to obtain solution C. Add 1.5g sodium chloride to solution C and stir for 120min to obtain solution D.

[0045] S2. Take a flat ceramic plate as a substrate, clean it with ultrasonic wave, dry it and place it at the bottom of the reactor. Place solution D in the reaction vessel. After 12 hours at 100°C, WO3 grows on the surface of the ceramic plate. Take out the ceramic plate, clean it and dry it to obtain a ceramic plate loaded with WO3.

[0046] Comparative Example 2

[0047] The preparation method of this comparative example is basically the same as that of Example 1, except that the pH in step S2 is controlled to be 2.0.

[0048] Comparative Example 3

[0049] The preparation method of this comparative example is basically the same as that of Example 1, except that the pH in step S2 is controlled to be 2.4.

[0050] The ceramic plate with WO3 / MGO nanocomposite material on the surface obtained in the above embodiment and the ceramic plate with WO3 obtained in comparative example 1 are used to assemble the sensor. The sensor is provided with a cylindrical protective shell on the outside, and the two sides of the shell are ceramic plates with WO3 / MGO grown on them, i.e., the flat ceramic plate 1 with WO3 / MGO nanocomposite material on the surface, as shown in FIG. Figure 5 As shown, as a gas-sensitive ceramic; a comb-shaped heating belt 2 is arranged inside the plate layer and fixed by the plate layer, and the root of the heating belt is connected to the foot seat and externally connected to the power supply. The arrangement of the comb-shaped heating belt can make the most efficient use of the bottom space of the ceramic plate and complete the heating of the ceramic plate with the highest efficiency.

[0051] The sensors based on the materials prepared in the above embodiment and comparative example 1 were used to detect triethylamine and formaldehyde gases respectively. The measuring circuit is shown in FIG. Figure 6 , just Figure 6 The gas-sensitive sintered body in the embodiment of the present invention is replaced with the above-mentioned sensor based on the ceramic plate carrying the WO3 / MGO nanocomposite material, and the sensor based on WO3 is used as a control example, that is, comparative example 1. The curve of its sensitivity changing with temperature is shown in the attached Figure 1 and Figure 2 .

[0052] By the attached Figure 1 and Figure 2 It can be seen that when the operating temperature is 180°C, the sensors of the embodiment and the control example both respond best to TEA, but WO3 compounded with MGO shows more excellent performance; when the operating temperature reaches 300°C, the sensors of the embodiment and the control example both respond best to CH2O, but WO3 compounded with MGO still shows more excellent performance.

[0053] In order to prevent the occurrence of cross-response at 180°C and 300°C, which may cause false alarm triggering, the two sensors were tested at two groups of working temperatures. It was found that at 180°C, the response of the two groups of sensors to TEA was much higher than that to CH2O, while at 300°C, it was just the opposite, indicating that no cross-alarm would be caused. Therefore, by controlling the working temperature to 180°C, the sensor of the present invention can be used to detect triethylamine gas; by controlling the working temperature to 180°C, the sensor of the present invention can be used to detect formaldehyde gas. That is, the same sensor can be used to detect triethylamine and formaldehyde gases by simply adjusting the working temperature, which reduces the replacement operation of the sensor and greatly improves the convenience of use.

[0054] The SEM images of the composite materials obtained in Comparative Examples 2 and 3 are shown in Figure 4 When the pH is controlled at 2.0 and 2.4, the composite material has poor morphology, small specific surface area and poor gas sensing performance. When the pH is controlled at 2.6, the prepared WO3 presents a nanorod shape. Figure 3 As shown, the morphology is uniform and the specific surface area is large, which is conducive to subsequent coating and performance improvement.

Claims

1. A method for preparing WO3 / MGO nanocomposite material, characterized in that: The steps include: Dissolve Na2WO4·2H2O in water to obtain solution A; slowly drop concentrated hydrochloric acid into solution A, stir after adding, and dilute with pure water to obtain solution B; add citric acid dihydrate to solution B until the pH of the solution reaches 2.6, stir, and dilute with water to obtain solution C; add sodium chloride to solution C to obtain solution D; Place the substrate in a reaction container, place solution D in the reaction container, control the temperature and time in the reaction container to allow WO3 to grow on the surface of the substrate; take out the substrate, wash it, and dry it for later use; The edge graphene oxide MGO treated at high temperature is dissolved in a solvent to prepare an MGO dispersion solution; the MGO dispersion solution and the substrate are placed in a reaction container, the temperature is controlled to perform a hydrothermal reaction, and after cooling to room temperature, the substrate is taken out, and after washing and drying, a composite material based on WO3 grown with MGO located on the surface of the substrate, namely, a WO3 / MGO nanocomposite material, is obtained.

2. The preparation method according to claim 1, characterized in that: The substrate is a ceramic plate.

3. The preparation method according to claim 1, characterized in that: The temperature of the high temperature treatment is 900-2500°C.

4. The preparation method according to claim 1, characterized in that: The temperature in the reaction container was controlled at 100°C to allow WO3 to grow on the surface of the substrate.

5. The preparation method according to claim 1, characterized in that: The solvent is ethanol.

6. The preparation method according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 200°C. 7.WO3 / MGO nanocomposite material, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 6.

8. The use of the WO3 / MGO nanocomposite material as claimed in claim 7, characterized in that: The method is used for preparing a gas sensor, wherein the WO3 / MGO nanocomposite material is used as a gas sensitive material and as a sensing layer material of the gas sensor.

9. The use according to claim 8, characterized in that: The gas sensor is used for detecting triethylamine and formaldehyde gases.

10. The use according to claim 9, characterized in that: When the operating temperature is 180°C, the gas sensor is used to detect triethylamine gas; when the operating temperature is 300°C, the gas sensor is used to detect formaldehyde gas.