Preparation method of Fe2 (MoO4) 3 / MoO3 nanosheet and application of Fe2 (MoO4) 3 / MoO3 nanosheet in detection of trimethylamine
The heterostructure of Fe2(MoO4)3/MoO3 nanosheets was prepared by solvent-thermal method and hydrothermal method, which solved the problem of insufficient sensing response and stability of MoO3 sensors in trimethylamine detection, and achieved high sensitivity and fast response trimethylamine Amines detection has a wide range of application prospects in early diagnosis of diseases and food safety testing.
Patent Information
- Application Number
- CN202410868032.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-01
AI Technical Summary
The existing MoO3 sensors still need to improve the sensing response, selectivity, stability and response/recovery time in trimethylamine detection, and the sensors have poor detection results under complex conditions.
The heterostructure of Fe2(MoO4)3/MoO3 nanosheets was prepared by solvothermal method combined with hydrothermal method. In which Fe2(MoO4)3 nanoparticles grew in situ on two-dimensional MoO3 nanosheets to prepare high-sensitivity trimethylamine detection materials .
It realizes high sensitivity detection of trimethylamine, including low concentration sensing response, excellent selectivity, good repeatability and fast response recovery time, and is suitable for early disease diagnosis and food safety testing.
Smart Images

Figure CN118877945A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of preparation and application of semiconductor gas-sensitive materials, and in particular to the preparation and application of Fe2(MoO4)3 / MoO3 flaky heterogeneous gas-sensitive materials. Background Art
[0002] Trimethylamine (TMA) is an important volatile organic compound widely used in the production of medicines, pesticides, dyes, and other organic synthetic materials. However, exposure to TMA through inhalation, ingestion, or skin absorption can cause various health problems, including dizziness, vomiting, nausea, coughing, and respiratory distress. To assess the freshness of seafood, TMA concentration is considered a reliable indicator, with levels below 10 ppm indicating freshness, 10-50 ppm indicating initial decay, and concentrations above 60 ppm indicating deep decay. In addition, the level of TMA in exhaled breath can be used as a biochemical marker for chronic kidney disease. Therefore, it is crucial to develop a highly sensitive detection method that can accurately measure trace amounts of TMA gas, which plays a vital role in protecting human health, protecting the environment, evaluating the freshness of seafood, and promoting medical diagnosis related to kidney disease. Compared with traditional technologies such as ion mobility spectrometry, mass spectrometry, gas chromatography, and infrared spectroscopy, metal oxide semiconductor (MOS) gas sensors are widely used for the detection of TMA due to their high cost-effectiveness, controllable manufacturing process, strong integration capability, small size, and high sensitivity.
[0003] To date, several MOS have been successfully applied in the field of gas sensors, including ZnO, WO3, In2O3, Fe2O3, and SnO2. Among these metal oxides, MoO3 has received great attention, especially in the detection of trimethylamine, due to the presence of abundant Lewis acid sites on the surface of MoO3, which facilitates the adsorption and activation of oxygen, thereby establishing a stable reaction basis with alkaline trimethylamine. However, the sensing response, selectivity, stability, and response / recovery time of MoO3 sensors still need further improvement. Since the gas sensing process in MOS sensors mainly relies on solid-gas interface reactions, the development of unique structures or interfaces has the potential to significantly improve the sensor performance. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing Fe2(MoO4)3 / MoO3 nanosheets and their application in trimethylamine detection. The present invention prepares a carefully designed Fe2(MoO4)3 / MoO3 heterostructure by combining a solvothermal method with a hydrothermal method, wherein Fe2(MoO4)3 nanoparticles are in situ grown on two-dimensional MoO3 nanosheets. The synthesized Fe2(MoO4)3 / MoO3 heterostructure is then used as a sensing material for detecting TMA. The Fe2(MoO4)3 / MoO3 heterostructure has potential practical application prospects in the fields of early disease diagnosis, food safety and detection under complex conditions.
[0005] The objective of the present invention is achieved through the following technical solutions: A method for preparing Fe2(MoO4)3 / MoO3 nanosheets, the preparation process and steps of the method: (1) Weigh a certain amount of ammonium molybdate tetrahydrate ((NH4)6Mo7O 24 ·4H2O), calcined at 500℃ for 2 h to obtain MoO3 precursor; (2) The MoO3 precursor prepared above was dissolved in H2O2 (30%) and stirred for 5 min, then methanol was added and stirred for 24 h, and ultrasonically treated at room temperature for 30 min. The solution was then transferred into a stainless steel autoclave lined with polytetrafluoroethylene and reacted at 180 °C for 12 h. (3) After the reactor cools down naturally, the powder is collected and washed three times by centrifugation with deionized water and ethanol respectively, and then placed in an oven overnight. Finally, the product is calcined at 400 °C for 2 h to obtain pure MoO3 nanosheet material. (4) Pure MoO3 nanosheets were dispersed in deionized water and ultrasonically treated for 1 h. Then, a certain amount of ferric chloride (FeCl3), sodium nitrate (NaNO3) and hydrochloric acid (HCl) were added and stirred until completely dissolved. The resulting mixture was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene and heated at 100°C for 8 h. After cooling to room temperature, it was washed several times with deionized water and ethanol and then dried at 60°C for 12 h.
[0006] (5) The dried product was placed in a clean crucible in a muffle furnace and calcined at 500 °C for 2 h to obtain Fe2(MoO4)3 / MoO3 nanosheets, which were then stored in a desiccator for analysis.
[0007] An application of Fe2(MoO4)3 / MoO3 nanosheet trimethylamine detection, Fe2(MoO4)3 / MoO3 nanosheet material is used as a gas sensitive material to make a gas sensor for the detection of trimethylamine gas: Firstly, Fe2(MoO4)3 / MoO3 nanosheets were added to anhydrous ethanol to make a uniform slurry, which was then coated on the outer wall of an alumina ceramic tube with two gold electrodes and four platinum wires. Then, a nickel-chromium heating wire was inserted into the ceramic tube. Finally, the four conductive wires of the ceramic tube and the two ends of the heating wire were welded to a six-pin base to obtain a gas sensor element. The gas sensitivity characteristics of the sensor were tested using a WS-30A gas sensitive tester. The test temperature was 25~350℃.
[0008] Advantages and beneficial effects of the present invention: In this paper, a well-designed Fe2(MoO4)3 / MoO3 heterostructure was prepared by a solvothermal method combined with a hydrothermal method, in which Fe2(MoO4)3 nanoparticles were grown in situ on two-dimensional MoO3 nanosheets. The synthesized Fe2(MoO4)3 / MoO3 heterostructure was then used as a sensing material for the detection of TMA. The results showed that the Fe2(MoO4)3 / MoO3 heterostructure had excellent sensitive properties to TMA, including very high sensing response even at low concentrations (0.1 ppm), excellent selectivity, good repeatability and stability, and very fast response recovery time. These findings suggest that the Fe2(MoO4)3 / MoO3 heterostructure has potential practical applications in the fields of early disease diagnosis, food safety, and detection under complex conditions.
[0009] (1) The present invention uses ammonium molybdate, ferric chloride, and sodium nitrate as raw materials to synthesize Fe2(MoO4)3 / MoO3 heterogeneous gas-sensitive materials by a solvothermal method combined with a hydrothermal method. The raw materials used in the experiment are cheap and easily available, and the production process is simple, which is suitable for industrial mass production.
[0010] (2) The present invention greatly improves the performance of the sensor by loading Fe2(MoO4)3 particles on MoO3 nanosheets for modification, and can detect trace amounts of trimethylamine in the air with high sensitivity and selectivity. In addition, the sensor has stable performance and is easy to prepare, and has broad application prospects in early disease diagnosis, food safety, and detection under complex conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 Schematic diagram of the structure of the trimethylamine sensor; Figure 2 It is the sensitivity of the gas sensor to 10 ppm trimethylamine gas at a test temperature of 25~350℃; Figure 3 The relationship between the trimethylamine concentration (0.1-200 ppm) and the response of the gas sensor at 200°C; Figure 4 is the selectivity of the gas sensor to 10 ppm gas at 200°C; Figure 5 is the response recovery curve of the gas sensor of Example 3 to 10 ppm trimethylamine gas at 200°C; Figure 6 This is the repeatability curve of the gas sensor of Example 3 at 200° C. for 10 ppm trimethylamine gas; Figure 7 This is a comparison diagram of the embodiments. DETAILED DESCRIPTION
[0012] The present invention will be described in detail below with reference to the embodiments shown in the accompanying drawings.
[0013] A method for preparing Fe2(MoO4)3 / MoO3 nanosheets, the method comprising the following preparation steps: Weigh a certain amount of (NH4)6Mo7O 24 4H2O, calcined at 500℃ for 2h to obtain MoO3 precursor; The MoO3 precursor prepared above was dissolved in H2O2 (30%) and stirred for 5 min, then methanol was added and stirred for 24 h, and ultrasonicated at room temperature for 30 min. The solution was then transferred into a stainless steel autoclave lined with polytetrafluoroethylene and reacted at 180 °C for 12 h. After the reactor cooled down naturally, the powder was collected, washed three times by centrifugation with deionized water and ethanol respectively, placed in an oven overnight, and finally calcined at 400 °C for 2 h to obtain pure MoO3 nanosheet material. Pure MoO3 nanosheets were dispersed in deionized water and ultrasonically treated for 1 h, and then a certain amount of FeCl3, NaNO3 and HCl were added and stirred until completely dissolved. The resulting mixture was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene and heated at 100°C for 8 h. After cooling to room temperature, it was washed several times with deionized water and ethanol, and then dried at 60°C for 12 h; The dried product was placed in a clean crucible in a muffle furnace and calcined at 500 °C for 2 h to obtain Fe2(MoO4)3 / MoO3 nanosheets, which were stored in a desiccator for analysis and detection. Example 1
[0014] Preparation of MoO3 nanosheets Step 1: Weigh 10.00 g (NH4)6Mo7O 24 4H2O, calcined at 500℃ for 2h to obtain MoO3 precursor; Step 2: Weigh 0.72 g of the MoO3 precursor obtained in step 1 and dissolve it in H2O2 (30%) and stir for 5 min. Then add methanol and stir for 24 h, and then ultrasonicate at room temperature for 30 min. Step 3: Transfer the solution from step 2 to a stainless steel autoclave lined with polytetrafluoroethylene, place it in an oven and heat it to 180°C for 12 h, and collect the powder after it cools down naturally; Step 4: The powder collected in step 3 is washed by centrifugation with deionized water and ethanol for three times, and then dried at 60°C for later use; Step 5: Place the precursor from step 4 directly into a muffle furnace and heat to 400 °C and maintain for 2 h to obtain pure MoO3 nanosheet material. Example 2
[0015] Preparation of 5-Fe2(MoO4)3 / MoO3 Nanosheets Steps 1, 2, 3, 4 and 5 are the same as in Example 1 Step 6: Disperse 0.150 g pure MoO3 nanosheets in deionized water, ultrasonicate for 1 h, then add 0.014 g FeCl3, 0.008 g NaNO3 and 30 μL HCl and stir until completely dissolved. Then transfer the resulting mixture to a stainless steel autoclave lined with polytetrafluoroethylene and heat at 100 ° C for 8 h. After cooling to room temperature, wash with deionized water and ethanol several times, and then dry at 60 ° C for 12 h; Step 7: Place the dried product in a clean crucible and place it in a muffle furnace, calcine at 500°C for 2 h to obtain 5-Fe2(MoO4)3 / MoO3 nanosheets, which are stored in a desiccator for analysis and detection. Example 3
[0016] Preparation of 10-Fe2(MoO4)3 / MoO3 nanosheets Steps 1, 2, 3, 4 and 5 are the same as in Example 1 Step 6: Disperse 0.150 g pure MoO3 nanosheets in deionized water, ultrasonicate for 1 h, then add 0.027 g FeCl3, 0.016 g NaNO3 and 30 μL HCl and stir until completely dissolved. Then transfer the resulting mixture to a stainless steel autoclave lined with polytetrafluoroethylene and heat at 100 ° C for 8 h. After cooling to room temperature, wash with deionized water and ethanol several times, and then dry at 60 ° C for 12 h; Step seven is the same as in Example 2. Example 4
[0017] Preparation of 15-Fe2(MoO4)3 / MoO3 Nanosheets Steps 1, 2, 3, 4 and 5 are the same as in Example 1 Step 6: Disperse 0.150 g pure MoO3 nanosheets in deionized water, ultrasonicate for 1 h, then add 0.040 g FeCl3, 0.024 g NaNO3 and 30 μL HCl and stir until completely dissolved. Then transfer the resulting mixture to a stainless steel autoclave lined with polytetrafluoroethylene and heat at 100 ° C for 8 h. After cooling to room temperature, wash with deionized water and ethanol several times, and then dry at 60 ° C for 12 h; Step seven is the same as in Example 2. Example 5
[0018] Preparation of 20-Fe2(MoO4)3 / MoO3 nanosheets Steps 1, 2, 3, 4 and 5 are the same as in Example 1 Step 6: Disperse 0.150 g pure MoO3 nanosheets in deionized water, ultrasonicate for 1 h, then add 0.054 g FeCl3, 0.032 g NaNO3 and 30 μL HCl and stir until completely dissolved. Then transfer the resulting mixture to a stainless steel autoclave lined with polytetrafluoroethylene and heat at 100 ° C for 8 h. After cooling to room temperature, wash with deionized water and ethanol several times, and then dry at 60 ° C for 12 h; Step seven is the same as in Example 2.
[0019] Gas Sensing Performance Test of Fe2(MoO4)3 / MoO3 Nanosheets Fe2(MoO4)3 / MoO3 nanosheets were added to anhydrous ethanol to make a slurry, which was coated on an Al2O3 ceramic tube, and then the ceramic tube and the nickel-chromium heating wire were welded on a six-legged base, as shown in Figure 1 As shown, a gas sensor element is manufactured. Figure 2 The figure shows the response of the sensor to 10 ppm trimethylamine gas at different operating temperatures (25-350°C). It can be seen from the figure that the response of the sensor increases with the increase of the operating temperature until the optimal operating temperature is reached. When the operating temperature continues to rise, the response of the sensor shows a downward trend. Among them, the optimal response value of the sensor in Example 1 is 9.14; the optimal response value of Example 2 is 40.36; the optimal response value of Example 3 is 85.35; the optimal response value of Example 4 is 43.24; the optimal response value of Example 5 is 25.90. It can be significantly found that the sensor in Example 3 has more significant sensing characteristics. Figure 3The dynamic response-recovery curve of the sensor to trimethylamine with a concentration of 0.1-200 ppm. As the concentration of trimethylamine increases, the response of the sensor also increases. When the concentration is 50 ppm, the response of the sensor is close to saturation. Remarkably, the response value of the sensor in Example 3 is the highest. When the concentration of trimethylamine is 10 ppm, the response is as high as 291.84. This result highlights its potential in detecting trimethylamine. Figure 4 The results of the sensor's selectivity test for various gases at 10 ppm are shown. It can be seen that the sensor has almost no response to interfering gases, which indicates that the sensor can selectively detect the presence of trimethylamine in a complex environment. Figure 5 The resistance curve of Example 3 to 10 ppm trimethylamine shows that the response and recovery time of Example 3 are 5 s and 71 s, respectively, which indicates that the sensor of Example 3 has strong recoverability. Figure 6 These are five dynamic response recovery cycles of the sensor of Example 3 under 10 ppm trimethylamine. The results show that the sensor of Example 3 has significant reversibility and reproducibility.
Claims
1. A method for preparing Fe2(MoO4)3 / MoO3 nanosheets, characterized in that: The process and steps of the method are as follows: (1) Weigh a certain amount of ammonium molybdate tetrahydrate ((NH4)6Mo7O 24 ·4H2O), calcined at 500℃ for 2 h to obtain MoO3 precursor; (2) The MoO3 precursor prepared above was dissolved in H2O2 (30%) and stirred for 5 min, then methanol was added and stirred for 24 h, and ultrasonically treated at room temperature for 30 min. The solution was then transferred into a stainless steel autoclave lined with polytetrafluoroethylene and reacted at 180 °C for 12 h. (3) After the reactor cools down naturally, the powder is collected and washed three times by centrifugation with deionized water and ethanol respectively, and then placed in an oven overnight. Finally, the product is calcined at 400 °C for 2 h to obtain pure MoO3 nanosheet material. (4) Pure MoO3 nanosheets were dispersed in deionized water and ultrasonically treated for 1 h. Then, a certain amount of ferric chloride (FeCl3), sodium nitrate (NaNO3) and hydrochloric acid (HCl) were added and stirred until completely dissolved. The resulting mixture was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene and heated at 100 °C for 8 h. After cooling to room temperature, it was washed several times with deionized water and ethanol, and then dried at 60 °C for 12 h. (5) The dried product was placed in a clean crucible in a muffle furnace and calcined at 500 °C for 2 h to obtain Fe2(MoO4)3 / MoO3 nanosheets, which were then stored in a desiccator for analysis.
2. An application of Fe2(MoO4)3 / MoO3 nanosheet trimethylamine detection, characterized in that: Fe2(MoO4)3 / MoO3 nanosheets are used as gas sensitive materials to make gas sensors for the detection of trimethylamine gas: Firstly, Fe2(MoO4)3 / MoO3 nanosheets were added to anhydrous ethanol to make a uniform slurry, which was then coated on the outer wall of an alumina ceramic tube with two gold electrodes and four platinum wires. Then, a nickel-chromium heating wire was inserted into the ceramic tube. Finally, the four conductive wires of the ceramic tube and the two ends of the heating wire were welded to a six-pin base to obtain a gas sensor element. The gas sensitivity characteristics of the sensor were tested using a WS-30A gas sensitive tester. The test temperature was 25~350℃.