3D printing hydrogel evaporator with temperature response and preparation method thereof
The hydrogel evaporator with temperature response was prepared through 3D printing technology, and materials such as sodium alginate and N-isopropyl acrylamide were used to solve the problems of traditional evaporators being susceptible to contamination and poor salt resistance, achieving efficient water Evaporation and salt discharge performance, suitable for seawater desalination and sewage treatment.
Patent Information
- Application Number
- CN202411128310.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-16
AI Technical Summary
Traditional hydrogel evaporators are easily contaminated due to their simple structure, especially the accumulation of salt, which leads to low evaporation efficiency or decrease in evaporation rate, making them difficult to make full use of light energy and poor salt resistance.
Using 3D printing technology to prepare a temperature-responsive hydrogel evaporator, using materials such as sodium alginate and N-isopropyl acrylamide, it is cured and molded through calcium chloride solution to form a porous interlaced structure and super hydrophilic functional unit. The layer realizes moisture transportation and photothermal response, improves evaporation efficiency and salt discharge performance.
It improves water evaporation efficiency and salt resistance, avoids pollution problems of traditional evaporators, enhances the light-thermal conversion performance and salt discharge capability of the device, and is suitable for seawater desalination and sewage treatment.
Smart Images

Figure CN118877992A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of seawater evaporation devices and relates to a 3D printed gel evaporator with temperature response and a preparation method thereof. Background Art
[0002] Distilling fresh water is an energy-intensive process, and sunlight under natural conditions can hardly meet the energy requirements for water evaporation. Hydrogel evaporators reduce the evaporation enthalpy of water by changing the interaction between polymers and water molecules, thereby avoiding the insufficient supply of solar energy.
[0003] However, traditional hydrogel evaporators have a simple structure, and water transport inside the device is limited by the microporous structure of the gel itself. They are easily contaminated after long-term use, especially salt accumulation, which seriously hinders the flow of liquid, causing serious problems such as low evaporation efficiency or decreased evaporation rate.
[0004] In order to make full use of light energy, improve photothermal conversion rate, enhance water evaporation efficiency and salt resistance, it is of great significance to develop gel devices with high salt resistance and high water evaporation efficiency. Summary of the invention
[0005] The purpose of the present invention is to at least partially solve the above technical problems, and to provide a temperature-responsive 3D printed hydrogel evaporator and a preparation method thereof. The 3D printed hydrogel evaporator prepared by the present invention has excellent light-to-heat conversion performance and water evaporation efficiency. The electrolyte properties of sodium alginate and the Marangoni effect caused by the spatial structure designed inside the device make the device have ultra-high salt removal performance, which is suitable for applications such as seawater desalination and sewage treatment.
[0006] In one aspect of the present invention, a 3D printed hydrogel evaporator with temperature response is provided, the 3D printed hydrogel evaporator comprising:
[0007] an evaporator upper layer, the evaporator upper layer being a photothermal response layer, the photothermal response layer comprising N-isopropylacrylamide as a thermosensitive polymer;
[0008] an evaporator lower layer, the evaporator lower layer being a hydrophilic layer configured to provide moisture to the evaporator upper layer,
[0009] The upper layer of the evaporator and the lower layer of the evaporator are adjusted in spatial structure through 3D printing technology and are integrally solidified.
[0010] In some embodiments, the integrated curing and molding is performed using a calcium chloride solution.
[0011] In some embodiments, the N-isopropylacrylamide undergoes a molecular conformational transition above the lower critical phase transition temperature, changing from hydrophilic to hydrophobic, and the molecular chain of the N-isopropylacrylamide changes from an extensible type to a contracted type to squeeze out water.
[0012] In some embodiments, the evaporator upper layer and the evaporator lower layer are configured as a porous staggered vertical and horizontal structure.
[0013] In some embodiments, the upper layer of the evaporator includes a plurality of super-hydrophilic functional sublayers prepared by 3D printing technology, each super-hydrophilic functional sublayer includes a plurality of elongated first gel cylinders spaced apart from each other;
[0014] The lower layer of the evaporator includes a plurality of super-hydrophilic functional sublayers prepared by 3D printing technology, and each super-hydrophilic functional sublayer includes a plurality of slender second gel cylinders spaced apart from each other;
[0015] The arrangement direction of the first gel cylinder and the second gel cylinder is an angle greater than 0 degrees and less than or equal to 90 degrees.
[0016] In some embodiments, water is transported between the first gel cylinders, between the second gel cylinders, and at the connection between the first gel cylinder and the second gel cylinder due to capillary action.
[0017] In another aspect of the present invention, a method for preparing the above-mentioned 3D printed hydrogel evaporator with temperature response is provided, and the preparation method comprises the following steps:
[0018] (1) adding 1 g of sodium alginate to 5-10 ml of water, and adding 50-100 mg of pyrrole and stirring to obtain a first solution, adding 0.1-1 g of polyvinyl alcohol and 0.1-0.5 g of potassium persulfate to 3 ml of deionized water, and stirring to obtain a second solution, and mixing the first solution and the second solution to obtain a first slurry;
[0019] (2) adding 1 g of sodium alginate to 5-10 ml of water, and adding 50-100 mg of pyrrole and stirring to obtain a third solution, adding 0.1-1 g of N-isopropylacrylamide and 10-30 mg of potassium persulfate to 3 ml of deionized water, stirring, heating at 60-80° C. and standing, and then adding 0.1-0.5 g of potassium persulfate and stirring to obtain a fourth solution, mixing the third solution and the fourth solution, and reacting at room temperature to obtain a second slurry;
[0020] (3) designing a three-dimensional model in SolidWorks software, wherein the three-dimensional model is printed with staggered lines, loading the first slurry and the second slurry into the barrel of the 3D printer respectively, importing the three-dimensional model into the 3D printer and starting printing;
[0021] (4) Print the first slurry and the second slurry into a device and add 0.5-2 mol / L CaCl 2 The solution is cured for 6 to 36 hours to obtain the temperature-responsive 3D printed hydrogel evaporator.
[0022] In some embodiments, in step (2), the heating time is 30-50 minutes, and the standing time is placing in a refrigerator at low temperature for 10-14 hours.
[0023] The reaction time at room temperature is 4-8 hours.
[0024] In some embodiments, in step (3), when staggered lines are printed, the spacing between upper lines is set to 0.1-0.5 mm, and the spacing between lower lines is set to 0.1-0.5 mm.
[0025] In some embodiments, in step (4), the first slurry and the second slurry are printed into a device at a height ratio of 1:0.2.
[0026] In some embodiments, the sodium alginate, polyvinyl alcohol and pyrrole in the first slurry are printed to form the lower layer of the evaporator of the hydrophilic layer.
[0027] The sodium alginate, N-isopropylacrylamide and pyrrole in the second slurry are printed to form the upper layer of the evaporator as the photothermal response layer.
[0028] The 3D printing gel evaporator with temperature response and the preparation method thereof according to the embodiment of the present invention have at least one of the following advantages:
[0029] The embodiment of the present invention uses sodium alginate, polyvinyl alcohol and pyrrole to prepare the first slurry A, and uses sodium alginate, N-isopropylacrylamide and pyrrole to prepare the second slurry B. The spatial structure is adjusted by 3D printing technology, and the slurry is solidified and formed as a whole by calcium chloride solution. The first slurry A has (super) hydrophilic properties. As the lower layer of the evaporator, it can provide moisture to the upper layer of the evaporator in time. The second slurry B is used as a photothermal response layer, in which poly N-isopropylacrylamide is a thermosensitive polymer. When its low critical phase transition temperature (about 32°C) is above, the molecular conformation changes from hydrophilic to hydrophobic, and the molecular chain changes from stretchability to curled type, squeezing out water, increasing the thickness of the evaporated water layer, reducing the interaction between water and the interface, and being more conducive to evaporation.
[0030] In addition, under light, poly (N-isopropylacrylamide) randomly divides the evaporation layer hydrogel into countless small areas. These small areas are composed of two parts with different temperatures. The hydrophobic structure has a higher temperature than the adjacent hydrophilic structure (evaporation absorbs heat). The temperature difference can effectively change the air convection above the interface, accelerate gas escape, and promote water evaporation.
[0031] Furthermore, the gel evaporator is 3D printed, and its internal space is controllable. Multiple water transport channels are established (the hydrogel itself can transport water, and the hydrogel lines can also transport water due to capillary action), breaking the limitation of traditional hydrogel water transport by the internal pores of the hydrogel itself, triggering the Marangoni effect, giving the device excellent salt removal performance, avoiding pore blockage and reduced evaporation efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] These and / or other aspects and advantages of the present invention will become apparent and readily understood from the following description of the preferred embodiments in conjunction with the accompanying drawings, in which:
[0033] Figure 1 is a structural model diagram of a 3D printed hydrogel evaporator with temperature response according to an embodiment of the present invention;
[0034] Figure 2 yes Figure 1 Marangoni effect diagram showing the temperature response of a 3D printed hydrogel evaporator;
[0035] Figure 3 For each embodiment of the present invention, 100 mw / cm 2 The actual picture of the 3D printed hydrogel evaporator after 8 hours of light exposure to test the salt removal ability. DETAILED DESCRIPTION
[0036] The technical solution of the present invention is further specifically described below by examples and in conjunction with the accompanying drawings. In the specification, the same or similar reference numerals indicate the same or similar components. The following description of the embodiments of the present invention with reference to the accompanying drawings is intended to explain the overall inventive concept of the present invention and should not be construed as a limitation of the present invention.
[0037] See also Figure 1 As the technical problem raised in the background technology section, an embodiment of the present invention provides a 3D printed hydrogel evaporator with temperature response, and the 3D printed hydrogel evaporator includes:
[0038] an evaporator upper layer, the evaporator upper layer being a photothermal response layer, the photothermal response layer comprising N-isopropylacrylamide as a thermosensitive polymer;
[0039] an evaporator lower layer, the evaporator lower layer being a hydrophilic layer configured to provide moisture to the evaporator upper layer,
[0040] The upper layer of the evaporator and the lower layer of the evaporator are adjusted in spatial structure through 3D printing technology and are integrally solidified.
[0041] The integrated curing and molding is performed by using a calcium chloride solution, wherein the concentration of the calcium chloride solution is 0.5 to 2 mol / L. Of course, those skilled in the art may also select other suitable solutions for the curing and molding.
[0042] Specifically, the N-isopropylacrylamide undergoes a molecular conformational transition above the lower critical phase transition temperature, changing from hydrophilic to hydrophobic, and the molecular chain of the N-isopropylacrylamide changes from an extensible type to a contracted type to squeeze out water.
[0043] In the present invention, the upper layer of the evaporator and the lower layer of the evaporator are arranged as a porous staggered vertical and horizontal structure.
[0044] In addition, under light, poly (N-isopropylacrylamide) randomly divides the evaporation layer hydrogel into countless small areas. These small areas are composed of two parts with different temperatures. The hydrophobic structure has a higher temperature than the adjacent hydrophilic structure (evaporation absorbs heat). The temperature difference can effectively change the air convection above the interface, accelerate gas escape, and promote water evaporation.
[0045] The multi-space staggered crisscross structure can be formed as follows:
[0046] The upper layer of the evaporator includes a plurality of super-hydrophilic functional sublayers prepared by 3D printing technology, and each super-hydrophilic functional sublayer includes a plurality of slender first gel cylinders spaced apart from each other;
[0047] The lower layer of the evaporator includes a plurality of super-hydrophilic functional sublayers prepared by 3D printing technology, and each super-hydrophilic functional sublayer includes a plurality of slender second gel cylinders spaced apart from each other;
[0048] The arrangement direction of the first gel cylinder and the second gel cylinder is an angle greater than 0 degrees and less than or equal to 90 degrees. Water is transported between the first gel cylinders, between the second gel cylinders, and at the connection between the first gel cylinder and the second gel cylinder due to capillary action.
[0049] Furthermore, the gel evaporator is 3D printed, and its internal space is controllable. Multiple water transport channels are established (the hydrogel itself can transport water, and the hydrogel lines can also transport water due to capillary action), breaking the limitation of traditional hydrogel water transport by the internal pores of the hydrogel itself, triggering the Marangoni effect, giving the device excellent salt removal performance, avoiding pore blockage and reduced evaporation efficiency.
[0050] See also Figure 2 , showing a diagram of the Marangoni effect inside a temperature-responsive 3D printed hydrogel evaporator.
[0051] The Marangoni effect describes the flow of fluid from a low surface tension area to a high surface tension area. The main cause of the Marangoni effect is the concentration gradient or temperature gradient. Figure 2 As can be seen in the figure, the temperature of the evaporator rises from A to B, forming a temperature gradient, and the water vapor moves upward. The salt concentration rises from A to B, forming a concentration gradient, and the water vapor refluxes, thus forming a vertical water cycle. The salt concentration in the gel cylinder in the horizontal direction also has a concentration gradient due to evaporation and capillary action, thus forming a horizontal water cycle.
[0052] An embodiment of the present invention also provides a method for preparing a 3D printed hydrogel evaporator with temperature response, the preparation method comprising the following steps:
[0053] (1) adding 1 g of sodium alginate to 5-10 ml of water, and adding 50-100 mg of pyrrole and stirring to obtain a first solution, adding 0.1-1 g of polyvinyl alcohol and 0.1-0.5 g of potassium persulfate to 3 ml of deionized water, and stirring to obtain a second solution, and mixing the first solution and the second solution to obtain a first slurry;
[0054] (2) adding 1 g of sodium alginate to 5-10 ml of water, and adding 50-100 mg of pyrrole and stirring to obtain a third solution, adding 0.1-1 g of N-isopropylacrylamide and 10-30 mg of potassium persulfate to 3 ml of deionized water, stirring, heating at 60-80° C. and standing, and then adding 0.1-0.5 g of potassium persulfate and stirring to obtain a fourth solution, mixing the third solution and the fourth solution, and reacting at room temperature to obtain a second slurry;
[0055] (3) designing a three-dimensional model in SolidWorks software, wherein the three-dimensional model is printed with staggered lines, loading the first slurry and the second slurry into the barrel of the 3D printer respectively, importing the three-dimensional model into the 3D printer and starting printing;
[0056] (4) Print the first slurry and the second slurry into a device and add 0.5-2 mol / L CaCl 2 The solution is cured for 6 to 36 hours to obtain the temperature-responsive 3D printed hydrogel evaporator.
[0057] In step (2), the heating time is 30-50 minutes, and the standing time is placing in a refrigerator at low temperature for 10-14 hours.
[0058] The reaction time at room temperature is 4-8 hours.
[0059] In step (3), when staggered lines are printed, the spacing between the upper layer lines is set to 0.1 to 0.5 mm, and the spacing between the lower layer lines is set to 0.1 to 0.5 mm.
[0060] In step (4), the first slurry and the second slurry are printed into a device at a height ratio of 1:0.2.
[0061] The sodium alginate, polyvinyl alcohol and pyrrole in the first slurry are printed to form the lower layer of the evaporator of the hydrophilic layer,
[0062] The sodium alginate, N-isopropylacrylamide and pyrrole in the second slurry are printed to form the upper layer of the evaporator as the photothermal response layer.
[0063] As described above, in the embodiment of the present invention, two different 3D printing slurries, namely the first slurry A and the second slurry B, are prepared, and the first slurry A and the second slurry B are 3D printed to form an upper and lower layer integrally solidified. 3 As an example, the following is described in conjunction with the preferred embodiment, and a device printed with a single first slurry A and a second slurry B is used as an example for comparison. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the invention, rather than limiting the claims of the invention. The described embodiments are only some embodiments of the invention, rather than all embodiments.
[0064] Example 1 (only the first slurry A)
[0065] (1) Add 1g of sodium alginate to 10ml of water, and add 100mg of pyrrole and stir evenly. Add 0.5g of polyvinyl alcohol and 0.1g of potassium persulfate to 3ml of deionized water and stir evenly. Mix the two solutions evenly to prepare a slurry.
[0066] (2) Design a 3D model in SolidWorks software, set the upper line spacing to 0.3mm, the lower line spacing to 0.1mm, and the upper layer thickness to lower layer thickness ratio to 1:0.2. Import the 3D model into the 3D printer and start printing. Print as 1*1*1cm 3 The device was filled with 1 mol / L CaCl 2 Cured in solution for 24 hours. 2 The evaporation efficiency of the evaporator was tested under simulated sunlight. The test results are shown in Table 1.
[0067] Example 2 (Second Slurry B Only)
[0068] (1) Add 1g of sodium alginate to 10ml of water, and add 100mg of pyrrole and stir evenly, which is called liquid a. Add 0.3g of N-isopropylacrylamide and 20mg of potassium persulfate to 3ml of deionized water, stir evenly, heat at 70℃ for 40mins, and put in the refrigerator for 12 hours. Then add 0.1g of potassium persulfate, which is called liquid b. After mixing liquid a and liquid b, react at room temperature for 6 hours to make the second slurry B.
[0069] (2) Design a 3D model in SolidWorks software, set the spacing between the upper layer of the slurry to 0.3 mm, and the spacing between the lower layer of the slurry to 0.1 mm. The ratio of the upper layer to the lower layer is 1:0.2, import the 3D model into the 3D printer and start printing.
[0070] (3) Print the slurry into 1*1*1cm 3 The device was filled with 1 mol / L CaCl 2 Cured in solution for 24 hours. 2 The evaporation efficiency of the evaporator was tested under simulated sunlight. The test results are shown in Table 1.
[0071] Example 3
[0072] (1) Add 1 g of sodium alginate to 10 ml of water, and add 100 mg of pyrrole and stir evenly. Add 0.5 g of polyvinyl alcohol and 0.1 g of potassium persulfate to 3 ml of deionized water and stir evenly. Mix the two solutions evenly to obtain the first slurry A.
[0073] (2) Add 1g of sodium alginate to 10ml of water and add 100mg of pyrrole, which is referred to as liquid a. Add 0.3g of N-isopropylacrylamide and 20mg of potassium persulfate to 3ml of deionized water, stir evenly, heat in a water bath at 70°C for 40mins, and place in a refrigerator for 12 hours. Then add 0.1g of potassium persulfate, which is referred to as liquid b. Mix liquids a and b, and react at room temperature for 6 hours to obtain the second slurry B.
[0074] (3) Design a 3D model in SolidWorks software, set the line spacing of slurry A to 0.1 mm, and the line spacing of slurry B to 0.2 mm. Import the 3D model into the 3D printer and start printing.
[0075] (4) Print the A and B slurries in a height ratio of 1:0.2 to 1*1*1cm 3 device and put in 1 mol / L CaCl 2 Curing in solution for 24 hours. 2 The evaporation efficiency of the evaporator was tested under simulated sunlight. The test results are shown in Table 1.
[0076] Example 4
[0077] (1) Add 1 g of sodium alginate to 7 ml of water, and add 100 mg of pyrrole and stir evenly. Add 0.5 g of polyvinyl alcohol and 0.1 g of potassium persulfate to 3 ml of deionized water and stir evenly. Mix the two solutions evenly to obtain the first slurry A.
[0078] (2) Add 1g of sodium alginate to 10ml of water and 100mg of pyrrole, which is referred to as liquid a. Add 0.3g of N-isopropylacrylamide and 20mg of potassium persulfate to 3ml of deionized water, stir evenly, heat in a water bath at 70°C for 40mins, and place in a refrigerator for 12 hours. Then add 0.1g of potassium persulfate, which is referred to as liquid b. Mix liquids a and b, and react at room temperature for 6 hours to obtain the second slurry B.
[0079] (3) Design a 3D model in SolidWorks software, set the line spacing of A slurry printing to 0.1 mm, and the line spacing of B slurry printing to 0.1 mm. Import the 3D model into the 3D printer and start printing.
[0080] (4) Print the first slurry A and the second slurry B in a height ratio of 1:0.2 to 1*1*1cm 3 device and put in 1 mol / L CaCl 2 Curing in solution for 24 hours. 2 The evaporation efficiency of the evaporator was tested under simulated sunlight. The test results are shown in Table 1.
[0081] Example 5
[0082] (1) Add 1 g of sodium alginate to 10 ml of water, and add 100 mg of pyrrole and stir evenly. Add 0.5 g of polyvinyl alcohol and 0.1 g of potassium persulfate to 3 ml of deionized water and stir evenly. Mix the two solutions evenly to obtain the first slurry A.
[0083] (2) Add 1g of sodium alginate to 10ml of water and add 100mg of pyrrole, which is referred to as liquid a. Add 0.3g of N-isopropylacrylamide and 20mg of potassium persulfate to 3ml of deionized water, stir evenly, heat in a water bath at 70°C for 40mins, and place in a refrigerator for 12 hours. Then add 0.1g of potassium persulfate, which is referred to as liquid b. Mix liquids a and b, and react at room temperature for 6 hours to obtain the second slurry B.
[0084] (3) Design a 3D model in SolidWorks software, set the line spacing of the first slurry A to 0.1 mm, and the line spacing of the second slurry B to 0.1 mm. Import the 3D model into the 3D printer and start printing.
[0085] (4) Print the first slurry A and the second slurry B in a height ratio of 1:0.2 to 1*1*1cm 3 device and put in 1 mol / L CaCl 2 Curing in solution for 24 hours. 2 The evaporation efficiency of the evaporator was tested under simulated sunlight. The test results are shown in Table 1.
[0086] Example 6
[0087] (1) Add 1 g of sodium alginate to 10 ml of water, and add 100 mg of pyrrole and stir evenly. Add 0.5 g of polyvinyl alcohol and 0.1 g of potassium persulfate to 3 ml of deionized water and stir evenly. Mix the two solutions evenly to obtain the first slurry A.
[0088] (2) Add 1g of sodium alginate to 10ml of water and add 100mg of pyrrole, which is referred to as liquid a. Add 0.4g of N-isopropylacrylamide and 20mg of potassium persulfate to 3ml of deionized water, stir evenly, heat in a water bath at 70°C for 40mins, and place in a refrigerator for 12 hours. Then add 0.1g of potassium persulfate, which is referred to as liquid b. Mix liquids a and b, and react at room temperature for 6 hours to obtain the second slurry B.
[0089] (3) Design a 3D model in SolidWorks software, set the line spacing of the first slurry A to 0.1 mm, and the line spacing of the second slurry B to 0.1 mm. Import the 3D model into the 3D printer and start printing.
[0090] (4) Print the first slurry A and the second slurry B in a height ratio of 1:0.2 to 1*1*1cm 3 device and put in 1 mol / L CaCl 2 Curing in solution for 24 hours.
[0091] By 1mw / cm 2 The evaporation efficiency of the evaporator was tested under simulated sunlight. The test results are shown in Table 1.
[0092] Table 1 Evaporation efficiency of seawater (3.5% brine) in Examples 1 to 6
[0093]
[0094] Table 2 Evaporation efficiency of concentrated brine (20% brine) in Examples 1 to 6
[0095]
[0096] The 3D printing gel evaporator with temperature response and the preparation method thereof according to the embodiment of the present invention have at least one of the following advantages:
[0097] The embodiment of the present invention uses sodium alginate, polyvinyl alcohol and pyrrole to prepare the first slurry A, and uses sodium alginate, N-isopropylacrylamide and pyrrole to prepare the second slurry B. The spatial structure is adjusted by 3D printing technology, and the slurry is solidified and formed as a whole by calcium chloride solution. The first slurry A has (super) hydrophilic properties. As the lower layer of the evaporator, it can provide moisture to the upper layer of the evaporator in time. The second slurry B is used as a photothermal response layer, in which poly N-isopropylacrylamide is a thermosensitive polymer. When its low critical phase transition temperature (about 32°C) is above, the molecular conformation changes from hydrophilic to hydrophobic, and the molecular chain changes from stretchability to curled type, squeezing out water, increasing the thickness of the evaporated water layer, reducing the interaction between water and the interface, and being more conducive to evaporation.
[0098] In addition, under light, poly (N-isopropylacrylamide) randomly divides the evaporation layer hydrogel into countless small areas. These small areas are composed of two parts with different temperatures. The hydrophobic structure has a higher temperature than the adjacent hydrophilic structure (evaporation absorbs heat). The temperature difference can effectively change the air convection above the interface, accelerate gas escape, and promote water evaporation.
[0099] Furthermore, the gel evaporator is 3D printed, and its internal space is controllable. Multiple water transport channels are established (the hydrogel itself can transport water, and the hydrogel lines can also transport water due to capillary action), breaking the limitation of traditional hydrogel water transport by the internal pores of the hydrogel itself, triggering the Marangoni effect, giving the device excellent salt removal performance, avoiding pore blockage and reduced evaporation efficiency.
[0100] Although some embodiments of the present general inventive concept have been shown and described, it will be appreciated by those skilled in the art that changes may be made to these embodiments without departing from the principles and spirit of the present general inventive concept, the scope of which is defined by the claims and their equivalents.
Claims
1. A 3D printed hydrogel evaporator with temperature response, characterized in that: The 3D printed hydrogel evaporator comprises: an evaporator upper layer, the evaporator upper layer being a photothermal response layer, the photothermal response layer comprising N-isopropylacrylamide as a thermosensitive polymer; an evaporator lower layer, the evaporator lower layer being a hydrophilic layer configured to provide moisture to the evaporator upper layer, The upper layer of the evaporator and the lower layer of the evaporator are adjusted in spatial structure through 3D printing technology and are integrally solidified.
2. The temperature-responsive 3D printed hydrogel evaporator according to claim 1, characterized in that: The integrated curing and molding is performed by using a calcium chloride solution.
3. The temperature-responsive 3D printed hydrogel evaporator according to claim 2, characterized in that: The N-isopropylacrylamide undergoes a molecular conformational change above the lower critical phase transition temperature, changing from hydrophilic to hydrophobic, and the molecular chain of the N-isopropylacrylamide changes from an extensible type to a contracted type to squeeze out water.
4. The temperature-responsive 3D printed hydrogel evaporator according to any one of claims 1 to 3, characterized in that: The upper layer of the evaporator and the lower layer of the evaporator are arranged in a porous staggered vertical and horizontal structure.
5. The temperature-responsive 3D printed hydrogel evaporator according to claim 4, characterized in that: The upper layer of the evaporator includes a plurality of super-hydrophilic functional sublayers prepared by 3D printing technology, and each super-hydrophilic functional sublayer includes a plurality of slender first gel cylinders spaced apart from each other; The lower layer of the evaporator includes a plurality of super-hydrophilic functional sublayers prepared by 3D printing technology, and each super-hydrophilic functional sublayer includes a plurality of slender second gel cylinders spaced apart from each other; The arrangement direction of the first gel cylinder and the second gel cylinder is an angle greater than 0 degrees and less than or equal to 90 degrees.
6. The temperature-responsive 3D printed hydrogel evaporator according to claim 5, characterized in that: Water is transported between the first gel cylinders, between the second gel cylinders, and at the connection between the first gel cylinder and the second gel cylinder due to capillary action.
7. A method for preparing a temperature-responsive 3D printed hydrogel evaporator according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) adding 1 g of sodium alginate to 5-10 ml of water, and adding 50-100 mg of pyrrole and stirring to obtain a first solution, adding 0.1-1 g of polyvinyl alcohol and 0.1-0.5 g of potassium persulfate to 3 ml of deionized water, and stirring to obtain a second solution, and mixing the first solution and the second solution to obtain a first slurry; (2) adding 1 g of sodium alginate to 5-10 ml of water, and adding 50-100 mg of pyrrole and stirring to obtain a third solution, adding 0.1-1 g of N-isopropylacrylamide and 10-30 mg of potassium persulfate to 3 ml of deionized water, stirring, heating at 60-80° C. and standing, and then adding 0.1-0.5 g of potassium persulfate and stirring to obtain a fourth solution, mixing the third solution and the fourth solution, and reacting at room temperature to obtain a second slurry; (3) designing a three-dimensional model in SolidWorks software, wherein the three-dimensional model is printed with staggered lines, loading the first slurry and the second slurry into the barrel of the 3D printer respectively, importing the three-dimensional model into the 3D printer and starting printing; (4) Printing the first slurry and the second slurry into devices, and placing them in a 0.5-2 mol / L CaCl2 solution for curing for 6-36 hours to obtain the temperature-responsive 3D printed hydrogel evaporator.
8. The preparation method according to claim 7, characterized in that: In step (2), the heating time is 30-50 minutes, and the standing time is placing in a refrigerator at low temperature for 10-14 hours. The reaction time at room temperature is 4-8 hours.
9. The preparation method according to claim 8, characterized in that: In step (3), when staggered lines are printed, the spacing between the upper layer lines is set to 0.1 to 0.5 mm, and the spacing between the lower layer lines is set to 0.1 to 0.5 mm.
10. The preparation method according to claim 9, characterized in that: In step (4), the first slurry and the second slurry are printed into a device at a height ratio of 1:0.2; The sodium alginate, polyvinyl alcohol and pyrrole in the first slurry are printed to form the lower layer of the evaporator of the hydrophilic layer, The sodium alginate, N-isopropylacrylamide and pyrrole in the second slurry are printed to form the upper layer of the evaporator as the photothermal response layer.
Citation Information
Patent Citations
Hydrogel driver containing nanometer microspheres, and preparation method and application of hydrogel driver
CN111909304A
Temperature-responsive high-strength hydrogel as well as preparation method and application thereof
CN115558132A
Novel self-adaptive evaporative cooling passive evaporative cooler and preparation method thereof
CN116379830A
Three-dimensional hydrogel tube photo-thermal conversion solar evaporator and preparation method and application thereof
CN117105314A
Preparation method of light-operated self-water-absorbing / water-releasing intelligent hydrogel
CN117362734A