Fluorine removal agent as well as preparation method and application thereof
By modifying the combination of concave and convex rods and polyhydroxycarboxylic acid-monomer salt blends, a porous structure adsorbent is formed, which solves the problems of low efficiency and high cost of existing fluorine-removing agents in the treatment of low concentration organic wastewater, and realizes the Efficient and economical fluoride ion removal effect.
Patent Information
- Application Number
- CN202411149505.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The existing fluorine-depleting agents are inefficient when treating fluorine-containing wastewater with low concentrations of organic matter, and have high preparation costs, making it difficult to meet the needs of industrial applications.
Using modified concave and convex rods and polyhydroxycarboxylic acid-monomer salt blends loaded on their surface, the copolymer chelates complexed by polyhydroxycarboxylic acid modification and porous structure adsorption and complexation can enhance fluorine removal ability and improve fluorine ions. Contact area and removal efficiency.
It has achieved efficient removal of fluorine-containing wastewater with low concentrations of organic matter, reduced preparation costs, and has the characteristics of thorough removal, small amount of sludge, economical and efficient, and stable compliance. It is suitable for the treatment of various fluoride-containing wastewater, and meets the requirements of green and environmental protection. .
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sewage treatment and relates to a defluorinating agent, in particular to a defluorinating agent and a preparation method and application thereof. Background Art
[0002] Fluorine is an element that is widely present in nature and has obvious biological toxicity. When the fluorine content in water exceeds the standard, it will not only threaten the survival of aquatic organisms and destroy the ecological balance, but also have serious effects on human health, such as causing tooth decay, weakening bone structure and strength, and damaging the nervous system and immune system. Excessive fluorine content in industrial wastewater, especially wastewater discharge from industries such as metallurgy, semiconductors, pharmaceuticals, chemicals, and material manufacturing, is the main cause of fluorine pollution in water bodies. With the rapid development of these industrial fields, the discharge of fluorine-containing wastewater has continued to increase, resulting in increasingly serious fluorine pollution in water bodies. Therefore, it is urgent to pay attention to and strengthen the treatment of fluorine-containing wastewater.
[0003] The chemical method of adding defluoridation agents to fluoride-containing wastewater to remove fluoride ions is the main means of treating fluoride-containing wastewater. This method is favored due to its high efficiency, easy operation and low cost, and has broad application prospects. At present, commonly used defluoridation agents mainly include various calcium salts, aluminum salts and magnesium salts, as well as composite agents made by mixing these salts with auxiliary materials. These composite agents mainly remove fluoride ions by chemical precipitation, that is, converting fluoride ions in water into insoluble fluoride, and then removing them by precipitation.
[0004] Although existing defluoridation agents are effective in treating high-concentration fluoride-containing wastewater (fluoride ion concentration ranges from tens to hundreds of milligrams per liter), they are often unsatisfactory in treating low-concentration fluoride-containing wastewater (fluoride ion concentration ranges from a few milligrams to more than ten milligrams per liter). In particular, when the wastewater contains a certain amount of organic matter, these organic matter will easily react with the defluoridation agent, further reducing the efficiency of treating low-concentration fluoride-containing wastewater.
[0005] It can be seen that how to provide a defluorination agent and a preparation method thereof to effectively treat low-concentration fluorine-containing wastewater containing organic matter, improve the defluorination efficiency, and reduce the preparation cost has become an urgent problem that technical personnel in this field need to solve. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a defluorinating agent and a preparation method and application thereof. The defluorinating agent includes a modified attapulgite and a polyhydroxycarboxylic acid-monomer salt blend loaded on the surface of the modified attapulgite, which can effectively treat low-concentration fluorine-containing wastewater containing organic matter, improve the defluorination efficiency, and reduce the preparation cost, which is conducive to large-scale promotion and application.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing a defluorination agent, the preparation method comprising the following steps:
[0009] (1) modifying the attapulgite ore with polyhydroxycarboxylic acid to obtain modified attapulgite;
[0010] (2) mixing the modified attapulgite, the hydroxycarboxylic acid compound, the monomer salt inorganic nanomaterial, the plasticizer, the storage agent, the dispersant and the deionized water, and stirring them uniformly to obtain an intermediate solution;
[0011] (3) adding a magnesium hydroxide aqueous solution to the intermediate solution until the pH value of the solution reaches the target value, and then solidifying, washing and drying are performed in sequence to obtain the defluorination agent.
[0012] The present invention modifies the attapulgite with polyhydroxycarboxylic acid, so that abundant active sites are formed on the modified surface, and the active sites can chemically adsorb with fluorine ions, thereby enhancing the defluorination ability; on this basis, hydroxycarboxylic acid compounds and monomer salt inorganic nanomaterials are mixed, and long-chain polyhydroxycarboxylic acid and porous structure adsorption and complex copolymer chelate are formed through the synergistic effect of multiple components, and the specific surface area and pore volume are further increased, which is conducive to increasing the contact area with fluorine ions in wastewater. The porous structure adsorption and complexation groups achieve the purpose of strong adsorption and flocculation sedimentation to efficiently remove fluoride in water, and have the characteristics of thorough removal, small amount of sludge, economical and efficient, and stable compliance with standards, and are suitable for the treatment of various fluoride-containing wastewaters, meeting green environmental protection requirements, and the long-chain polyhydroxycarboxylic acid has good organic compatibility, and even in wastewater containing organic matter, the defluoridation agent can effectively react with fluorine ions, thereby avoiding the negative impact of organic matter on defluorination efficiency, and having broad application prospects.
[0013] Preferably, the polyhydroxycarboxylic acid modification in step (1) comprises the following steps:
[0014] (1.1) dispersing the attapulgite ore in deionized water to remove impurities, and filtering to obtain the first attapulgite;
[0015] (1.2) dispersing the first attapulgite in a hydrochloric acid solution for acid treatment, filtering, washing, drying and crushing in sequence to obtain a second attapulgite;
[0016] (1.3) The second attapulgite is dispersed in deionized water, and sodium pentahydroxycaproate is added, and the temperature is first raised to a first temperature for evaporation treatment, and then the temperature is raised to a second temperature for pressure polymerization reaction, and the modified attapulgite is obtained after filtering.
[0017] Since the attapulgite ore contains impurities such as quartz and carbonate during the formation process, and the presence of these impurities will have an adverse effect on the fluorine removal performance of the attapulgite, the present invention fully removes the above impurities through sequential impurity removal and acid treatment, thereby further improving the fluorine removal performance of the attapulgite.
[0018] Preferably, the concentration of the hydrochloric acid solution in step (1.2) is 0.5-1 mol / L, for example, it can be 0.5 mol / L, 0.55 mol / L, 0.6 mol / L, 0.65 mol / L, 0.7 mol / L, 0.75 mol / L, 0.8 mol / L, 0.85 mol / L, 0.9 mol / L, 0.95 mol / L or 1 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0019] Preferably, the acid treatment time in step (1.2) is 1.5-2.5 h, for example, 1.5 h, 1.6 h, 1.7 h, 1.8 h, 1.9 h, 2 h, 2.1 h, 2.2 h, 2.3 h, 2.4 h or 2.5 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] Preferably, the mixing mass ratio of the sodium pentahydroxycaproate and the second attapulgite in step (1.3) is (0.3-0.5):1, for example, it can be 0.3:1, 0.32:1, 0.34:1, 0.36:1, 0.38:1, 0.4:1, 0.42:1, 0.44:1, 0.46:1, 0.48:1 or 0.5:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, the first temperature in step (1.3) is 100-110°C, for example, it can be 100°C, 101°C, 102°C, 103°C, 104°C, 105°C, 106°C, 107°C, 108°C, 109°C or 110°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] Preferably, the time for the evaporation treatment in step (1.3) is 30-60 min, for example, it can be 30 min, 32 min, 34 min, 36 min, 38 min, 40 min, 42 min, 44 min, 46 min, 48 min, 50 min, 52 min, 54 min, 56 min, 58 min or 60 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0023] Preferably, the second temperature in step (1.3) is 140-160°C, for example, it can be 140°C, 142°C, 144°C, 146°C, 148°C, 150°C, 152°C, 154°C, 156°C, 158°C or 160°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, the absolute pressure of the pressurized polymerization reaction in step (1.3) is 0.2-0.4 MPa, for example, it can be 0.2 MPa, 0.22 MPa, 0.24 MPa, 0.26 MPa, 0.28 MPa, 0.3 MPa, 0.32 MPa, 0.34 MPa, 0.36 MPa, 0.38 MPa or 0.4 MPa, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] Preferably, the time for the pressurized polymerization reaction in step (1.3) is 30-60 min, for example, it can be 30 min, 32 min, 34 min, 36 min, 38 min, 40 min, 42 min, 44 min, 46 min, 48 min, 50 min, 52 min, 54 min, 56 min, 58 min or 60 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the hydroxycarboxylic acid compound in step (2) comprises sodium pentahydroxyhexanoate and / or polyhydroxyalkanoate.
[0027] Preferably, the degree of polymerization of the polyhydroxyalkanoate is 30-100, for example, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95 or 100, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] Preferably, the monomer salt inorganic nanomaterial in step (2) comprises any one of sodium salt, aluminum salt, iron salt or magnesium salt, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of sodium salt and aluminum salt, a combination of aluminum salt and iron salt, a combination of iron salt and magnesium salt, a combination of sodium salt, aluminum salt and iron salt, or a combination of aluminum salt, iron salt and magnesium salt.
[0029] Preferably, the plasticizer in step (2) comprises any one of lignin sulfonate, polycarboxylic acid, naphthalene sulfonate, aromatic aminosulfonate or sulfonated melamine formaldehyde resin, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of lignin sulfonate and polycarboxylic acid, a combination of polycarboxylic acid and naphthalene sulfonate, a combination of naphthalene sulfonate and aromatic aminosulfonate, or a combination of aromatic aminosulfonate and sulfonated melamine formaldehyde resin.
[0030] Preferably, the storage agent in step (2) includes zirconium oxychloride and / or zirconium oxide.
[0031] Preferably, the dispersant in step (2) comprises polyisobutylene succinimide.
[0032] Preferably, the mixing mass ratio of the modified attapulgite, hydroxycarboxylic acid compound, monomer salt inorganic nanomaterial, plasticizer, storage agent and dispersant in step (2) is (20-30):(15-25):(10-20):(2-5):(3-6):(1-4), for example, it can be 20:15:10:2:3:1, 22:17:12:2:3:1, 24:19:14:3:4:2, 26:21:16:4:5:3, 28:23:18:5:6:4 or 30:25:20:5:6:4, and further preferably is (23-27):(18-22):(12-16):(3-4):(4-5):(2-3), but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0033] Preferably, the target pH value of the solution in step (3) is 7-9, for example, 7, 7.2, 7.4, 7.6, 7.8, 8, 8.2, 8.4, 8.6, 8.8 or 9, more preferably 8-9, but not limited to the listed values, other values not listed within the numerical range are also applicable.
[0034] Preferably, the drying method in step (3) includes freeze drying or heat drying.
[0035] Preferably, the heating and drying temperature is 75-85°C, for example, it can be 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C or 85°C, and the time is 2-3h, for example, it can be 2h, 2.1h, 2.2h, 2.3h, 2.4h, 2.5h, 2.6h, 2.7h, 2.8h, 2.9h or 3h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] As a preferred technical solution of the first aspect of the present invention, the preparation method comprises the following steps:
[0037] (1) Modifying the attapulgite ore into polyhydroxycarboxylic acid, specifically comprising:
[0038] (1.1) dispersing the attapulgite ore in deionized water to remove impurities, and filtering to obtain the first attapulgite;
[0039] (1.2) dispersing the first attapulgite in a 0.5-1 mol / L hydrochloric acid solution and subjecting it to acid treatment for 1.5-2.5 h, filtering, washing, drying and crushing in sequence to obtain a second attapulgite;
[0040] (1.3) dispersing the second attapulgite in deionized water, and adding sodium pentahydroxycaproate, controlling the mixing mass ratio of sodium pentahydroxycaproate and the second attapulgite to be (0.3-0.5):1, first heating to 100-110° C. for evaporation treatment for 30-60 min, then heating to 140-160° C., and performing a pressure polymerization reaction at 0.2-0.4 MPa for 30-60 min, and filtering to obtain the modified attapulgite;
[0041] (2) Mixing modified attapulgite, hydroxycarboxylic acid compound, monomer salt inorganic nanomaterial, plasticizer, storage agent, dispersant and deionized water, stirring evenly to obtain an intermediate solution; the hydroxycarboxylic acid compound includes sodium pentahydroxycaproate and / or polyhydroxyalkanoate, and the degree of polymerization of the polyhydroxyalkanoate is 30-100; the monomer salt inorganic nanomaterial includes any one of sodium salt, aluminum salt, iron salt or magnesium salt or a combination of at least two; the plasticizer includes any one of lignin sulfonate, polycarboxylic acid, naphthalene sulfonate, aromatic aminosulfonate or sulfonated melamine formaldehyde resin or a combination of at least two; the storage agent includes zirconium oxychloride and / or zirconium oxide; the dispersant includes polyisobutylene succinimide; the mixed mass ratio of the modified attapulgite, hydroxycarboxylic acid compound, monomer salt inorganic nanomaterial, plasticizer, storage agent and dispersant is (23-27):(18-22):(12-16):(3-4):(4-5):(2-3);
[0042] (3) adding a magnesium hydroxide aqueous solution to the intermediate solution until the pH value of the solution reaches 8-9, and sequentially solidifying, washing and drying to obtain the defluorinating agent; the drying method includes freeze drying or heating drying, and the heating drying temperature is 75-85° C. and the time is 2-3 hours.
[0043] In a second aspect, the present invention provides a defluorinating agent, which is prepared by the preparation method described in the first aspect, and comprises a modified attapulgite and a polyhydroxycarboxylic acid-monomer salt blend loaded on the surface of the modified attapulgite.
[0044] In a third aspect, the present invention provides a use of the defluorination agent as described in the second aspect in treating fluoride-containing wastewater.
[0045] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] The present invention modifies the attapulgite with polyhydroxycarboxylic acid, so that abundant active sites are formed on the modified surface, and the active sites can chemically adsorb with fluorine ions, thereby enhancing the defluorination ability; on this basis, hydroxycarboxylic acid compounds and monomer salt inorganic nanomaterials are mixed, and long-chain polyhydroxycarboxylic acid and porous structure adsorption and complex copolymer chelate are formed through the synergistic effect of multiple components, and the specific surface area and pore volume are further increased, which is conducive to increasing the contact area with fluorine ions in wastewater. The porous structure adsorption and complexation groups achieve the purpose of strong adsorption and flocculation sedimentation to efficiently remove fluoride in water, and have the characteristics of thorough removal, small amount of sludge, economical and efficient, and stable compliance with standards, and are suitable for the treatment of various fluoride-containing wastewaters, meeting green environmental protection requirements, and the long-chain polyhydroxycarboxylic acid has good organic compatibility, and even in wastewater containing organic matter, the defluoridation agent can effectively react with fluorine ions, thereby avoiding the negative impact of organic matter on defluorination efficiency, and having broad application prospects. DETAILED DESCRIPTION
[0048] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0049] Example 1
[0050] This embodiment provides a defluorination agent and a preparation method thereof, the preparation method comprising the following steps:
[0051] (1) Modifying the attapulgite ore into polyhydroxycarboxylic acid, specifically comprising:
[0052] (1.1) dispersing the attapulgite ore in deionized water to remove impurities, and filtering to obtain the first attapulgite;
[0053] (1.2) dispersing the first attapulgite in a 0.8 mol / L hydrochloric acid solution and subjecting it to an acid treatment for 1.5 h, and then filtering, washing, drying and crushing the attapulgite in sequence to obtain a second attapulgite;
[0054] (1.3) dispersing the second attapulgite in deionized water, and adding sodium pentahydroxycaproate, controlling the mixing mass ratio of sodium pentahydroxycaproate and the second attapulgite to be 0.4:1, first heating to 105° C. for evaporation treatment for 45 min, then heating to 150° C., and performing pressure polymerization reaction at 0.4 MPa for 45 min, and filtering to obtain a modified attapulgite;
[0055] (2) mixing 23 parts of modified attapulgite, 18 parts of sodium pentahydroxycaproate, 12 parts of sodium sulfate, 3 parts of sodium lignin sulfonate, 4 parts of zirconium oxychloride, 2 parts of polyisobutylene succinimide (with a degree of polymerization of 6000-10000) and deionized water, and stirring to obtain an intermediate solution;
[0056] (3) adding a magnesium hydroxide aqueous solution to the intermediate solution until the pH value of the solution reaches 8, and then solidifying, washing and freeze-drying in sequence to obtain the defluorination agent.
[0057] The defluorination agent obtained in this embodiment includes modified attapulgite and a polyhydroxycarboxylic acid-monomer salt blend loaded on the surface of the modified attapulgite, forming a copolymer chelate with long-chain polyhydroxycarboxylic acid and porous structure adsorption and complexation.
[0058] Example 2
[0059] This embodiment provides a defluorination agent and a preparation method thereof, the preparation method comprising the following steps:
[0060] (1) Modifying the attapulgite ore into polyhydroxycarboxylic acid, specifically comprising:
[0061] (1.1) dispersing the attapulgite ore in deionized water to remove impurities, and filtering to obtain the first attapulgite;
[0062] (1.2) dispersing the first attapulgite in a 0.5 mol / L hydrochloric acid solution and subjecting it to an acid treatment for 1.5 h, and then filtering, washing, drying and crushing it in sequence to obtain a second attapulgite;
[0063] (1.3) dispersing the second attapulgite in deionized water, and adding sodium pentahydroxycaproate, controlling the mixing mass ratio of sodium pentahydroxycaproate and the second attapulgite to be 0.3:1, first heating to 100° C. for evaporation treatment for 60 min, then heating to 140° C., and performing pressure polymerization reaction at 0.4 MPa for 60 min, and filtering to obtain modified attapulgite;
[0064] (2) mixing 27 parts of modified attapulgite, 22 parts of polyhydroxyalkanoate (with a degree of polymerization of 30-100), 16 parts of magnesium sulfate, 4 parts of sodium naphthalenesulfonate, 5 parts of zirconium oxide, 3 parts of polyisobutylene succinimide (with a degree of polymerization of 6000-10000) and deionized water, and stirring to obtain an intermediate solution;
[0065] (3) A magnesium hydroxide aqueous solution is added dropwise to the intermediate solution until the pH value of the solution reaches 9, and the solution is solidified, washed and heated to dry (temperature is 85° C., time is 2 h) in sequence to obtain the defluorination agent.
[0066] The defluorination agent obtained in this embodiment includes modified attapulgite and a polyhydroxycarboxylic acid-monomer salt blend loaded on the surface of the modified attapulgite, forming a copolymer chelate with long-chain polyhydroxycarboxylic acid and porous structure adsorption and complexation.
[0067] Example 3
[0068] This embodiment provides a defluorination agent and a preparation method thereof, the preparation method comprising the following steps:
[0069] (1) Modifying the attapulgite ore into polyhydroxycarboxylic acid, specifically comprising:
[0070] (1.1) dispersing the attapulgite ore in deionized water to remove impurities, and filtering to obtain the first attapulgite;
[0071] (1.2) dispersing the first attapulgite in a 1 mol / L hydrochloric acid solution and subjecting it to an acid treatment for 2.5 h, and then filtering, washing, drying and crushing it in sequence to obtain a second attapulgite;
[0072] (1.3) dispersing the second attapulgite in deionized water, and adding sodium pentahydroxycaproate, controlling the mixing mass ratio of sodium pentahydroxycaproate and the second attapulgite to be 0.3:1, first heating to 110° C. for evaporation treatment for 30 min, then heating to 160° C., and performing a pressure polymerization reaction at 0.3 MPa for 30 min, and filtering to obtain a modified attapulgite;
[0073] (2) mixing 20 parts of modified attapulgite, 15 parts of sodium pentahydroxycaproate, 10 parts of ferric nitrate, 2 parts of sodium naphthalenesulfonate, 3 parts of zirconium oxychloride, 1 part of polyisobutylene succinimide (with a degree of polymerization of 6000-10000) and deionized water, and stirring to obtain an intermediate solution;
[0074] (3) A magnesium hydroxide aqueous solution is added dropwise to the intermediate solution until the pH value of the solution reaches 7, and the solution is solidified, washed and heated to dry (temperature is 75° C., time is 3 h) in sequence to obtain the defluorination agent.
[0075] The defluorination agent obtained in this embodiment includes modified attapulgite and a polyhydroxycarboxylic acid-monomer salt blend loaded on the surface of the modified attapulgite, forming a copolymer chelate with long-chain polyhydroxycarboxylic acid and porous structure adsorption and complexation.
[0076] Example 4
[0077] This embodiment provides a defluorination agent and a preparation method thereof. Except for deleting step (1.2), that is, the attapulgite is not subjected to acid treatment, the remaining steps and conditions are the same as those in Example 1, and thus are not described in detail here.
[0078] Example 5
[0079] This embodiment provides a defluorinating agent and a preparation method thereof. Except that only a pressure polymerization reaction is performed in step (1.3) without evaporation treatment before that, the remaining steps and conditions are the same as those in Example 1, and thus will not be described in detail here.
[0080] Comparative Example 1
[0081] This comparative example provides a defluorination agent and a preparation method thereof. Except that the attapulgite ore is not modified with polyhydroxycarboxylic acid, the remaining steps and conditions are the same as those in Example 1, and thus are not described in detail here.
[0082] Comparative Example 2
[0083] This comparative example provides a defluorination agent and a preparation method thereof. Except that sodium sulfate is not added in step (2), the remaining steps and conditions are the same as those in Example 1, and thus are not described in detail here.
[0084] Comparative Example 3
[0085] This comparative example provides a defluorination agent and a preparation method thereof. Except that sodium lignin sulfonate is not added in step (2), the remaining steps and conditions are the same as those in Example 1, and thus are not described in detail here.
[0086] Comparative Example 4
[0087] This comparative example provides a defluorination agent and a preparation method thereof. Except that zirconium oxychloride is not added in step (2), the remaining steps and conditions are the same as those in Example 1, and thus are not described in detail here.
[0088] Comparative Example 5
[0089] This comparative example provides a defluorination agent and a preparation method thereof. Except that polyisobutylene succinimide is not added in step (2), the remaining steps and conditions are the same as those in Example 1, and thus are not described in detail here.
[0090] Performance Testing
[0091] 10 groups of fluorine-containing organic wastewater were prepared, and the pH of the wastewater was controlled to be 6, the fluorine ion concentration was 10 mg / L, and the chemical oxygen demand COD was 500 mg / L. The defluorinating agents obtained in Examples 1-5 and Comparative Examples 1-5 were added to the above 10 groups of fluorine-containing organic wastewater, and the added amount was 10 g. The defluorinating agents were fully stirred to make them suspended and fully contact with the fluorine-containing organic wastewater. After stirring for 5 hours, the residual fluorine ion concentration in the wastewater was detected. The relevant test results are shown in Table 1 below.
[0092] Table 1
[0093] Fluoride removal agent Residual fluoride ion concentration (mg / L) Fluoride removal efficiency (%) Example 1 0.129 98.71 Example 2 0.142 98.58 Example 3 0.135 98.65 Example 4 2.137 78.63 Example 5 2.351 76.49 Comparative Example 1 1.568 84.32 Comparative Example 2 1.383 86.17 Comparative Example 3 1.154 88.46 Comparative Example 4 1.302 86.98 Comparative Example 5 1.542 84.58
[0094] It can be seen that the present invention modifies the attapulgite with polyhydroxycarboxylic acid, so that abundant active sites are formed on the modified surface, and these active sites can chemically adsorb with fluoride ions, thereby enhancing the defluorination ability; on this basis, hydroxycarboxylic acid compounds and monomer salt inorganic nanomaterials are mixed, and long-chain polyhydroxycarboxylic acids and porous structure adsorption and complex copolymer chelates are formed through the synergistic effect of multiple components, which further increases the specific surface area and pore volume, which is beneficial to increase the contact area with fluoride ions in wastewater, and the porous structure adsorption and complexing groups achieve the purpose of strong adsorption and flocculation sedimentation to efficiently remove fluoride in water, and have the characteristics of thorough removal, small amount of sludge, economical and efficient, and stable compliance, suitable for the treatment of various types of fluoride-containing wastewater, meet the requirements of green environmental protection, and long-chain polyhydroxycarboxylic acids have good compatibility with organic matter, even in wastewater containing organic matter, the defluoridation agent can effectively react with fluoride ions, thereby avoiding the negative impact of organic matter on the defluorination efficiency, and has broad application prospects.
[0095] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a defluorinating agent, characterized in that: The preparation method comprises the following steps: (1) modifying the attapulgite ore with polyhydroxycarboxylic acid to obtain modified attapulgite; (2) mixing the modified attapulgite, the hydroxycarboxylic acid compound, the monomer salt inorganic nanomaterial, the plasticizer, the storage agent, the dispersant and the deionized water, and stirring them uniformly to obtain an intermediate solution; (3) adding a magnesium hydroxide aqueous solution to the intermediate solution until the pH value of the solution reaches the target value, and then solidifying, washing and drying are performed in sequence to obtain the defluorination agent.
2. The preparation method according to claim 1, characterized in that: The polyhydroxycarboxylic acid modification in step (1) comprises the following steps: (1.1) dispersing the attapulgite ore in deionized water to remove impurities, and filtering to obtain the first attapulgite; (1.2) dispersing the first attapulgite in a hydrochloric acid solution for acid treatment, filtering, washing, drying and crushing in sequence to obtain a second attapulgite; (1.3) The second attapulgite is dispersed in deionized water, and sodium pentahydroxycaproate is added, and the temperature is first raised to a first temperature for evaporation treatment, and then the temperature is raised to a second temperature for pressure polymerization reaction, and the modified attapulgite is obtained after filtering.
3. The preparation method according to claim 2, characterized in that: The concentration of the hydrochloric acid solution in step (1.2) is 0.5-1 mol / L; Preferably, the acid treatment time in step (1.2) is 1.5-2.5h; Preferably, the mixing mass ratio of the sodium pentahydroxycaproate and the second attapulgite in step (1.3) is (0.3-0.5):
1.
4. The preparation method according to claim 2 or 3, characterized in that: Step (1.3) the first temperature is 100-110°C; Preferably, the evaporation treatment time in step (1.3) is 30-60 min; Preferably, the second temperature in step (1.3) is 140-160°C; Preferably, the absolute pressure of the pressurized polymerization reaction in step (1.3) is 0.2-0.4 MPa; Preferably, the time for the pressurized polymerization reaction in step (1.3) is 30-60 minutes.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The hydroxycarboxylic acid compound in step (2) includes sodium pentahydroxyhexanoate and / or polyhydroxyalkanoate; Preferably, the degree of polymerization of the polyhydroxyalkanoate is 30-100; Preferably, the monomer salt inorganic nanomaterial in step (2) comprises any one of sodium salt, aluminum salt, iron salt or magnesium salt, or a combination of at least two thereof; Preferably, the plasticizer in step (2) comprises any one or a combination of at least two of lignin sulfonate, polycarboxylic acid, naphthalene sulfonate, aromatic aminosulfonate or sulfonated melamine formaldehyde resin; Preferably, the storage agent in step (2) comprises zirconium oxychloride and / or zirconium oxide; Preferably, the dispersant in step (2) comprises polyisobutylene succinimide.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The mixing mass ratio of the modified attapulgite, hydroxycarboxylic acid compound, monomer salt inorganic nanomaterial, plasticizer, storage agent and dispersant in step (2) is (20-30): (15-25): (10-20): (2-5): (3-6): (1-4), and is further preferably (23-27): (18-22): (12-16): (3-4): (4-5): (2-3).
7. The preparation method according to any one of claims 1 to 6, characterized in that: The target pH value of the solution in step (3) is 7-9, more preferably 8-9; Preferably, the drying method in step (3) includes freeze drying or heat drying; Preferably, the heating and drying is carried out at a temperature of 75-85°C and for a time of 2-3 hours.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) Modifying the attapulgite ore into polyhydroxycarboxylic acid, specifically comprising: (1.1) dispersing the attapulgite ore in deionized water to remove impurities, and filtering to obtain the first attapulgite; (1.2) dispersing the first attapulgite in a 0.5-1 mol / L hydrochloric acid solution and subjecting it to acid treatment for 1.5-2.5 h, filtering, washing, drying and crushing in sequence to obtain a second attapulgite; (1.3) dispersing the second attapulgite in deionized water, and adding sodium pentahydroxycaproate, controlling the mixing mass ratio of sodium pentahydroxycaproate and the second attapulgite to be (0.3-0.5):1, first heating to 100-110° C. for evaporation treatment for 30-60 min, then heating to 140-160° C., and performing a pressure polymerization reaction at 0.2-0.4 MPa for 30-60 min, and filtering to obtain the modified attapulgite; (2) Mixing modified attapulgite, hydroxycarboxylic acid compound, monomer salt inorganic nanomaterial, plasticizer, storage agent, dispersant and deionized water, stirring evenly to obtain an intermediate solution; the hydroxycarboxylic acid compound includes sodium pentahydroxycaproate and / or polyhydroxyalkanoate, and the degree of polymerization of the polyhydroxyalkanoate is 30-100; the monomer salt inorganic nanomaterial includes any one of sodium salt, aluminum salt, iron salt or magnesium salt or a combination of at least two; the plasticizer includes any one of lignin sulfonate, polycarboxylic acid, naphthalene sulfonate, aromatic aminosulfonate or sulfonated melamine formaldehyde resin or a combination of at least two; the storage agent includes zirconium oxychloride and / or zirconium oxide; the dispersant includes polyisobutylene succinimide; the mixed mass ratio of the modified attapulgite, hydroxycarboxylic acid compound, monomer salt inorganic nanomaterial, plasticizer, storage agent and dispersant is (23-27):(18-22):(12-16):(3-4):(4-5):(2-3); (3) adding a magnesium hydroxide aqueous solution to the intermediate solution until the pH value of the solution reaches 8-9, and sequentially solidifying, washing and drying to obtain the defluorinating agent; the drying method includes freeze drying or heating drying, and the heating drying temperature is 75-85° C. and the time is 2-3 hours.
9. A defluorination agent, characterized in that: The defluorinating agent is prepared by the preparation method according to any one of claims 1 to 8, and comprises a modified attapulgite and a polyhydroxycarboxylic acid-monomer salt blend loaded on the surface of the modified attapulgite.
10. Use of the defluorination agent as claimed in claim 9 in treating fluoride-containing wastewater.
Citation Information
Patent Citations
Preparation method of attapulgite / zirconia composite defluorinating material
CN102247797A
Production method of attapulgite loaded hydroxyapatite composite defluorination filter bulb
CN102502907A
Fluorine removal agent, preparation method and fluorine removal method for hydrofluoric acid wastewater
CN114477564A
Fluorine removal agent for fluorine-containing wastewater treatment and preparation method thereof
CN117247092A
Production method of filter medium for removing fluoride from drinking water