Capillary crystallization type concrete waterproof material for airfield pavement and preparation method of capillary crystallization type concrete waterproof material
By using a combination of multiple solid waste and specific waterproof additives in airport road concrete, the high cost of waterproofing materials and solid waste problems of permeable crystalline concrete are solved, and efficient waterproofing performance and self-healing ability are achieved, reducing maintenance costs and environmental protection are achieved. threaten.
Patent Information
- Application Number
- CN202410934473.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-01
AI Technical Summary
The cost of permeable crystal masterbatch in existing permeable crystalline concrete waterproof materials is high and the solid waste storage is large, which affects the application and environmental protection needs of airport pavement projects.
Using multiple solid waste such as fly ash and slag as the basic materials, combined with active silicon waterproofing additives, complexing agents, waterproofing additives and calcium ion compensation agents, to form a crystalline concrete waterproofing material for the airport road surface, mixed by dry powder and stirring to improve waterproof and impermeability resistance and self-healing ability.
It has achieved the reduction of the production cost of waterproof materials, enhanced the performance and durability of concrete road surfaces, and has permanent self-repairing effect, improved compressive strength and chemical erosion resistance, significantly reduced crack healing width and maintenance costs.
Smart Images

Figure BDA0004940871200000091
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of airport pavement construction material application, and specifically relates to a method for preparing an airport pavement permeable crystalline concrete waterproof material using multi-component solid waste and a preparation method thereof. Background Art
[0002] Concrete is a common and widely used building material with advantages such as high strength and good durability. As the construction technology of concrete in airport pavement is mature and there is rich experience in engineering application, concrete pavement has also been widely used. Concrete pavement has high compressive strength and is suitable for bearing the heavy load brought by aircraft takeoff and landing. Due to its durability, the maintenance and repair frequency of concrete pavement is low, and the maintenance cost is low in the long run. However, due to the brittle nature of concrete itself, the concrete structure in the airport pavement is prone to microcracks in the structure due to factors such as temperature difference and stress during service. As the service time increases, the accumulation of stress will cause the microcracks to continue to expand and widen, and may even develop to penetrate the concrete structure. Structural cracking is a key factor affecting the normal use of airport pavement. The generation of cracks allows more harmful media to enter the concrete structure, constantly exchanging Ca(OH)2 dissolved in the concrete, causing the cracks to continue to increase, seriously affecting the concrete's impermeability and service life.
[0003] In response to this, there is a method of applying waterproof materials to the outside of concrete or paving the surface, which can improve the waterproof ability of concrete to a certain extent. However, aging and damage of such waterproof materials are inevitable, which means high repair costs. It is both time-consuming and laborious, and the waterproof reliability of such waterproof materials cannot be guaranteed. There is also a kind of penetrating crystallization waterproof material that can effectively solve the problem of concrete leakage; it can form structural waterproofing with the airport pavement, greatly improving the waterproof ability of concrete. The advantage of penetrating crystallization waterproof material is that it has self-repairing ability, which can make the airport pavement entity have permanent waterproof ability, which not only ensures the safe use of the structure within the design life, but also greatly reduces the high cost of maintenance.
[0004] However, the current domestic permeable crystallization concrete waterproofing materials mainly rely on imported permeable crystallization masterbatches for preparation; due to the high production cost of waterproofing materials caused by the import of masterbatches, the scope of its application in concrete waterproofing projects is limited. For domestic airport pavement projects, it is of great significance to develop a waterproofing material that can replace the imported permeable crystallization masterbatch. In addition, combined with the requirements of environmental protection policies, the large-scale storage of solid waste in my country poses a huge threat to the environment. Promoting the comprehensive utilization of solid waste is of great significance to improving resource utilization efficiency, improving environmental quality, and promoting the comprehensive green transformation of economic and social development. Therefore, combined with the current high cost of waterproofing materials and domestic environmental protection requirements, it is a topic of practical significance and value to study a method of using multiple solid waste to prepare airport pavement permeable crystallization concrete waterproofing materials, reduce costs, benefit environmental protection, and further enhance the performance and durability of concrete pavements. Summary of the invention
[0005] The purpose of the present invention is to provide an airport pavement permeable crystallization concrete waterproof material, which solves the problems of relatively high cost of permeable crystallization masterbatch and large stockpile of solid waste in the permeable crystallization concrete waterproof material in the prior art, reduces costs, is beneficial to environmental protection, and further enhances the performance and durability of concrete pavement; the present invention also provides a preparation method of the airport pavement permeable crystallization concrete waterproof material.
[0006] To achieve the above-mentioned purpose, the present invention provides an airport pavement permeable crystalline concrete waterproof material, which comprises at least the following components in parts by weight: 48-52 parts of cement, 15-20 parts of industrial solid waste, 30-35 parts of quartz sand, 0.25-0.75 parts of active silicon waterproofing agent, 0.2-0.4 parts of complexing agent, 0.1-0.3 parts of waterproofing agent, and 0.2-0.6 parts of calcium ion compensator.
[0007] Further preferably, the waterproof material includes at least the following components in parts by weight: 50 parts of cement, 18 parts of industrial solid waste, 30 parts of quartz sand, 0.25 parts of active silicon waterproofing agent, 0.2 parts of chelating agent, 0.1 parts of waterproofing agent, and 0.2 parts of calcium ion compensator.
[0008] Further preferably, the waterproof material includes at least the following components in parts by weight: 50 parts of cement, 18 parts of industrial solid waste, 30 parts of quartz sand, 0.5 parts of active silicon waterproofing agent, 0.2 parts of chelating agent, 0.3 parts of waterproofing agent, and 0.4 parts of calcium ion compensator.
[0009] Further preferably, the waterproof material includes at least the following components in parts by weight: 50 parts of cement, 18 parts of industrial solid waste, 30 parts of quartz sand, 0.75 parts of active silicon waterproofing agent, 0.2 parts of chelating agent, 0.2 parts of waterproofing agent, and 0.6 parts of calcium ion compensator.
[0010] Preferably, the industrial solid waste includes at least fly ash and slag, the weight ratio of fly ash to slag is 1-2:1, and the relative density of fly ash is 1.9-2.4 g / cm 3 , slag is ground to a specific surface area greater than 400m 2 / kg.
[0011] Further preferably, the cement is 42.5 ordinary Portland cement, and the particles with a particle size less than 5 μm in the cement account for 14%-16% of the total weight of the cement; the particle size of the quartz sand is 0.1-0.3 mm, and the mud content is 0.04%.
[0012] Further preferably, the active silicon waterproofing agent is a mixture of sodium methyl silicate and sodium aluminate in a weight ratio of 3:1.
[0013] Further preferably, the complexing agent is a mixture of glycine and calcium lignin sulfonate in a weight ratio of 2.5:1.
[0014] Further preferably, the waterproofing agent is a mixture of calcined coal gangue and desulfurized gypsum in a weight ratio of 1:1. The calcium ion compensator is steel slag powder.
[0015] The present invention also provides a method for preparing an airport pavement permeable crystalline concrete waterproof material, which is characterized in that the preparation method comprises the following steps:
[0016] S1. Mix 48-52 parts of cement, 15-20 parts of industrial solid waste and 30-35 parts of quartz sand in a dry powder mixer to obtain a premix A; the mixing time is 4-8 minutes;
[0017] S2. Add 0.25-0.75 parts of active silicon waterproofing agent, 0.2-0.4 parts of complexing agent, 0.1-0.3 parts of waterproofing agent and 0.2-0.6 parts of calcium ion compensator to the premix A obtained in step S1 in sequence; stir evenly to obtain the airport pavement permeable crystalline concrete waterproof material.
[0018] The airport pavement permeable crystalline concrete waterproof material of the present invention uses silicate cement and quartz sand as basic materials, and on the basis of ensuring its waterproof performance, industrial solid waste materials are added; combined with the application and compatibility of active silicon waterproofing additives, chelating agents, waterproofing additives, and calcium ion compensating agents, the waterproof and anti-seepage performance of the airport pavement permeable crystalline concrete waterproof material is improved, the self-healing ability of cracks in concrete is improved and enhanced, thereby further improving the mechanical properties and durability of concrete.
[0019] In the waterproof material of the present invention, the active silicon waterproofing agent can improve the penetration ability of the waterproof material in the cement-based material to achieve the effect of deep crystallization; at the same time, the active silicon waterproofing agent and the waterproofing agent can supplement the SO42-, AlO3-, SiO32- and other ions required for the crystallization reaction; the calcium ion compensator can supplement calcium ions for the concrete, and the common ion effect occurs in the concrete to promote the growth process of the crystal; the complexing agent can react with the partially dissolved Ca(OH)2 in the concrete to generate an unstable calcium ion complex. When the calcium ion complex diffuses with the water medium and encounters acid ions (such as silicate ions, aluminate ions, and carbonate ions), the calcium ion complex will be replaced with it to generate more stable calcium silicate gel, calcium aluminate and calcium carbonate crystals. After the insoluble crystals are generated, the complexing agent ions will restore the free radicals, continue to combine with Ca2+, and move Ca2+ to the cracks. The insoluble crystals continue to accumulate, intertwine, and overlap to expand to the entire space. The chemical components in the waterproof material interact with each other to improve the waterproof and anti-seepage properties of concrete.
[0020] The present invention has the following beneficial effects:
[0021] The permeable crystallization waterproof material of the present invention has a permanent self-repairing effect on concrete, and the maximum healing width can reach 0.54mm. The active chemical substances in the waterproof material are stable, do not decompose and do not age. When the concrete is in a dry environment, the complex substances in the waterproofing agent component are in a dormant state. When water invades, the complex in the waterproofing agent will be activated and react with the hydration product of cement to generate unstable calcium ion complexes. When encountering active silicon oxide, active aluminum oxide or silicate, the complex ions will be replaced to generate water-insoluble crystals. As the number of insoluble crystals increases, the crack space is continuously reduced until the crack heals. When the concrete is restored to dryness, the complex component is dormant again. Throughout the process, the complex component acts as a "porter" and continuously moves Ca2+ from high concentration to low concentration without consuming it. Thereby achieving a permanent self-repairing effect. The waterproof material of the present invention is added to concrete to improve the structural density and improve its mechanical properties. The compressive strength 28d and flexural strength can reach 48.6MPa and 9.2MPa respectively. The waterproof material of the present invention can also effectively reduce the penetration of chloride ions in concrete and improve the chemical corrosion resistance and crack resistance of concrete.
[0022] More importantly, part of the raw materials used in the present invention are derived from solid waste, which effectively reduces the production cost of waterproof materials, and takes into account the complementary characteristics of various components and optimizes the configuration. By adding fly ash and slag, and then adjusting the ratio of active silicon waterproofing additives, chelating agents, waterproofing additives, and calcium ion compensators, a low-cost airport pavement permeable crystalline concrete waterproof material with excellent waterproof and anti-seepage properties, durability and self-healing properties is obtained. DETAILED DESCRIPTION
[0023] The core of the present invention is to provide an airport pavement permeable crystallization concrete waterproof material, which solves the problems of relatively high cost of permeable crystallization masterbatch and large stockpile of solid waste in the permeable crystallization concrete waterproof material in the prior art, reduces costs, is beneficial to environmental protection, and further enhances the performance and durability of concrete pavement.
[0024] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the implementation modes.
[0025] Embodiment 1:
[0026] A permeable crystalline concrete waterproof material for airport pavement, the waterproof material comprises at least the following components by weight: 48 parts of 42.5 ordinary Portland cement, 15 parts of industrial solid waste, 30 parts of quartz sand, 0.25 parts of active silicon waterproofing agent, 0.2 parts of complexing agent, 0.1 parts of waterproofing agent, and 0.2 parts of calcium ion compensator. The 15 parts of industrial solid waste include 7.5 parts of fly ash and 7.5 parts of slag, the weight ratio of fly ash to slag is 1:1, and the relative density of fly ash is 1.9-2.4g / cm 3 , slag is ground to a specific surface area greater than 400m 2 / kg. In this embodiment, the particles with a particle size of less than 5 μm in the silicate cement account for 14-16% of the total weight of the cement; the particle size of the quartz sand is 0.1-0.3 mm, and the mud content is 0.04%; the active silicon waterproofing agent is a mixture of sodium methyl silicate and sodium metaaluminate at a weight ratio of 3:1; the complexing agent is a mixture of glycine and calcium lignin sulfonate at a weight ratio of 2.5:1; the waterproofing agent is a mixture of calcined coal gangue and desulfurized gypsum at a weight ratio of 1:1; and the calcium ion compensator is steel slag powder.
[0027] Embodiment 2:
[0028] A permeable crystalline concrete waterproof material for airport pavement, the waterproof material at least comprises the following components by weight: 52 parts of 42.5 ordinary Portland cement, 20 parts of industrial solid waste, 35 parts of quartz sand, 0.75 parts of active silicon waterproofing agent, 0.4 parts of complexing agent, 0.3 parts of waterproofing agent, and 0.6 parts of calcium ion compensator. The 20 parts of industrial solid waste include 10 parts of fly ash and 10 parts of slag, the weight ratio of fly ash to slag is 1:1, and the relative density of fly ash is 1.9-2.4g / cm 3 , slag is ground to a specific surface area greater than 400m 2 / kg. In this embodiment, the particles with a particle size of less than 5 μm in the silicate cement account for 14-16% of the total weight of the cement; the particle size of the quartz sand is 0.1-0.3 mm, and the mud content is 0.04%; the active silicon waterproofing agent is a mixture of sodium methyl silicate and sodium metaaluminate at a weight ratio of 3:1; the complexing agent is a mixture of glycine and calcium lignin sulfonate at a weight ratio of 2.5:1; the waterproofing agent is a mixture of calcined coal gangue and desulfurized gypsum at a weight ratio of 1:1; and the calcium ion compensator is steel slag powder.
[0029] Embodiment 3:
[0030] A permeable crystalline concrete waterproof material for airport pavement, the waterproof material comprises at least the following components by weight: 50 parts of 42.5 ordinary Portland cement, 18 parts of industrial solid waste, 30 parts of quartz sand, 0.25 parts of active silicon waterproofing agent, 0.4 parts of complexing agent, 0.3 parts of waterproofing agent, and 0.6 parts of calcium ion compensator. The 18 parts of industrial solid waste include 9 parts of fly ash and 9 parts of slag, the weight ratio of fly ash to slag is 1:1, and the relative density of fly ash is 1.9-2.4g / cm 3 , slag is ground to a specific surface area greater than 400m 2 / kg. In this embodiment, the particles with a particle size of less than 5 μm in the silicate cement account for 14-16% of the total weight of the cement; the particle size of the quartz sand is 0.1-0.3 mm, and the mud content is 0.04%; the active silicon waterproofing agent is a mixture of sodium methyl silicate and sodium metaaluminate at a weight ratio of 3:1; the complexing agent is a mixture of glycine and calcium lignin sulfonate at a weight ratio of 2.5:1; the waterproofing agent is a mixture of calcined coal gangue and desulfurized gypsum at a weight ratio of 1:1; and the calcium ion compensator is steel slag powder.
[0031] Embodiment 4:
[0032] A permeable crystalline concrete waterproof material for airport pavement, the waterproof material comprises at least the following components by weight: 50 parts of 42.5 ordinary Portland cement, 18 parts of industrial solid waste, 30 parts of quartz sand, 0.5 parts of active silicon waterproofing agent, 0.2 parts of complexing agent, 0.3 parts of waterproofing agent, and 0.4 parts of calcium ion compensator. The 18 parts of industrial solid waste include 9 parts of fly ash and 9 parts of slag, the weight ratio of fly ash to slag is 1:1, and the relative density of fly ash is 1.9-2.4g / cm 3 , slag is ground to a specific surface area greater than 400m 2 / kg. In this embodiment, the particles with a particle size of less than 5 μm in the silicate cement account for 14-16% of the total weight of the cement; the particle size of the quartz sand is 0.1-0.3 mm, and the mud content is 0.04%; the active silicon waterproofing agent is a mixture of sodium methyl silicate and sodium metaaluminate at a weight ratio of 3:1; the complexing agent is a mixture of glycine and calcium lignin sulfonate at a weight ratio of 2.5:1; the waterproofing agent is a mixture of calcined coal gangue and desulfurized gypsum at a weight ratio of 1:1; and the calcium ion compensator is steel slag powder.
[0033] Embodiment 5:
[0034] A permeable crystalline concrete waterproof material for airport pavement, the waterproof material comprises at least the following components by weight: 50 parts of 42.5 ordinary Portland cement, 18 parts of industrial solid waste, 30 parts of quartz sand, 0.5 parts of active silicon waterproofing agent, 0.3 parts of complexing agent, 0.1 parts of waterproofing agent, and 0.6 parts of calcium ion compensator. The 18 parts of industrial solid waste include 9 parts of fly ash and 9 parts of slag, the weight ratio of fly ash to slag is 1:1, and the relative density of fly ash is 1.9-2.4g / cm 3 , slag is ground to a specific surface area greater than 400m 2 / kg. In this embodiment, the particles with a particle size of less than 5 μm in the silicate cement account for 14-16% of the total weight of the cement; the particle size of the quartz sand is 0.1-0.3 mm, and the mud content is 0.04%; the active silicon waterproofing agent is a mixture of sodium methyl silicate and sodium metaaluminate at a weight ratio of 3:1; the complexing agent is a mixture of glycine and calcium lignin sulfonate at a weight ratio of 2.5:1; the waterproofing agent is a mixture of calcined coal gangue and desulfurized gypsum at a weight ratio of 1:1; and the calcium ion compensator is steel slag powder.
[0035] Embodiment 6:
[0036] A permeable crystalline concrete waterproof material for airport pavement, the waterproof material comprises at least the following components by weight: 50 parts of 42.5 ordinary Portland cement, 18 parts of industrial solid waste, 30 parts of quartz sand, 0.5 parts of active silicon waterproofing agent, 0.4 parts of complexing agent, 0.2 parts of waterproofing agent, and 0.2 parts of calcium ion compensator. The 18 parts of industrial solid waste include 9 parts of fly ash and 9 parts of slag, the weight ratio of fly ash to slag is 1:1, and the relative density of fly ash is 1.9-2.4g / cm 3 , slag is ground to a specific surface area greater than 400m 2 / kg. In this embodiment, the particles with a particle size of less than 5 μm in the silicate cement account for 14-16% of the total weight of the cement; the particle size of the quartz sand is 0.1-0.3 mm, and the mud content is 0.04%; the active silicon waterproofing agent is a mixture of sodium methyl silicate and sodium metaaluminate at a weight ratio of 3:1; the complexing agent is a mixture of glycine and calcium lignin sulfonate at a weight ratio of 2.5:1; the waterproofing agent is a mixture of calcined coal gangue and desulfurized gypsum at a weight ratio of 1:1; and the calcium ion compensator is steel slag powder.
[0037] Embodiment 7:
[0038] A permeable crystalline concrete waterproof material for airport pavement, the waterproof material at least comprises the following components by weight: 50 parts of 42.5 ordinary Portland cement, 18 parts of industrial solid waste, 30 parts of quartz sand, 0.75 parts of active silicon waterproofing agent, 0.2 parts of complexing agent, 0.2 parts of waterproofing agent, and 0.6 parts of calcium ion compensator. The 18 parts of industrial solid waste include 9 parts of fly ash and 9 parts of slag, the weight ratio of fly ash to slag is 1:1, and the relative density of fly ash is 1.9-2.4g / cm 3 , slag is ground to a specific surface area greater than 400m 2 / kg. In this embodiment, the particles with a particle size of less than 5 μm in the silicate cement account for 14-16% of the total weight of the cement; the particle size of the quartz sand is 0.1-0.3 mm, and the mud content is 0.04%; the active silicon waterproofing agent is a mixture of sodium methyl silicate and sodium metaaluminate at a weight ratio of 3:1; the complexing agent is a mixture of glycine and calcium lignin sulfonate at a weight ratio of 2.5:1; the waterproofing agent is a mixture of calcined coal gangue and desulfurized gypsum at a weight ratio of 1:1; and the calcium ion compensator is steel slag powder.
[0039] Embodiment 8:
[0040] A permeable crystalline concrete waterproof material for airport pavement, the waterproof material comprises at least the following components by weight: 50 parts of 42.5 ordinary Portland cement, 18 parts of industrial solid waste, 30 parts of quartz sand, 0.75 parts of active silicon waterproofing agent, 0.3 parts of complexing agent, 0.3 parts of waterproofing agent, and 0.2 parts of calcium ion compensator. The 18 parts of industrial solid waste include 9 parts of fly ash and 9 parts of slag, the weight ratio of fly ash to slag is 1:1, and the relative density of fly ash is 1.9-2.4g / cm 3 , slag is ground to a specific surface area greater than 400m 2 / kg. In this embodiment, the particles with a particle size of less than 5 μm in the silicate cement account for 14-16% of the total weight of the cement; the particle size of the quartz sand is 0.1-0.3 mm, and the mud content is 0.04%; the active silicon waterproofing agent is a mixture of sodium methyl silicate and sodium metaaluminate at a weight ratio of 3:1; the complexing agent is a mixture of glycine and calcium lignin sulfonate at a weight ratio of 2.5:1; the waterproofing agent is a mixture of calcined coal gangue and desulfurized gypsum at a weight ratio of 1:1; and the calcium ion compensator is steel slag powder.
[0041] Embodiment 9:
[0042] A permeable crystalline concrete waterproof material for airport pavement, the waterproof material comprises at least the following components by weight: 50 parts of 42.5 ordinary Portland cement, 18 parts of industrial solid waste, 30 parts of quartz sand, 0.75 parts of active silicon waterproofing agent, 0.4 parts of complexing agent, 0.1 parts of waterproofing agent, and 0.4 parts of calcium ion compensator. The 18 parts of industrial solid waste include 9 parts of fly ash and 9 parts of slag, the weight ratio of fly ash to slag is 1:1, and the relative density of fly ash is 1.9-2.4g / cm 3 , slag is ground to a specific surface area greater than 400m 2 / kg. In this embodiment, the particles with a particle size of less than 5 μm in the silicate cement account for 14-16% of the total weight of the cement; the particle size of the quartz sand is 0.1-0.3 mm, and the mud content is 0.04%; the active silicon waterproofing agent is a mixture of sodium methyl silicate and sodium metaaluminate at a weight ratio of 3:1; the complexing agent is a mixture of glycine and calcium lignin sulfonate at a weight ratio of 2.5:1; the waterproofing agent is a mixture of calcined coal gangue and desulfurized gypsum at a weight ratio of 1:1; and the calcium ion compensator is steel slag powder.
[0043] Embodiment 10:
[0044] A permeable crystalline concrete waterproof material for airport pavement, the waterproof material comprises at least the following components by weight: 50 parts of 42.5 ordinary Portland cement, 16 parts of industrial solid waste, 35 parts of quartz sand, 0.6 parts of active silicon waterproofing agent, 0.3 parts of complexing agent, 0.2 parts of waterproofing agent, and 0.5 parts of calcium ion compensator. The 16 parts of industrial solid waste include 8 parts of fly ash and 8 parts of slag, the weight ratio of fly ash to slag is 1:1, and the relative density of fly ash is 1.9-2.4g / cm 3 , slag is ground to a specific surface area greater than 400m 2 / kg. In this embodiment, the particles with a particle size of less than 5 μm in the silicate cement account for 14-16% of the total weight of the cement; the particle size of the quartz sand is 0.1-0.3 mm, and the mud content is 0.04%; the active silicon waterproofing agent is a mixture of sodium methyl silicate and sodium metaaluminate at a weight ratio of 3:1; the complexing agent is a mixture of glycine and calcium lignin sulfonate at a weight ratio of 2.5:1; the waterproofing agent is a mixture of calcined coal gangue and desulfurized gypsum at a weight ratio of 1:1; and the calcium ion compensator is steel slag powder.
[0045] Embodiment 11:
[0046] This embodiment provides a method for preparing the airport pavement permeable crystalline concrete waterproof material as in Embodiments 1-10, the preparation method comprising the following steps:
[0047] S1. Mix cement, industrial solid waste and quartz sand in parts by weight in any one of Examples 1 to 10 in a dry powder mixer to obtain a premix A; the mixing time is 4 to 8 minutes, preferably 5 minutes;
[0048] S2. Add the corresponding active silicon waterproofing agent, chelating agent, waterproofing agent and calcium ion compensator in Examples 1-10 to the premix A obtained in step S1 in sequence; stir evenly to obtain the airport pavement permeable crystalline concrete waterproofing material.
[0049] Comparative Example 1:
[0050] A permeable crystalline concrete waterproof material for airport pavement prepared by utilizing multiple solid wastes, which does not contain active silicon waterproofing aid, chelating agent, waterproofing aid, or calcium ion compensating agent, and the rest is the same as in Example 1.
[0051] The relevant performances of Examples 1-10 and Comparative Example 1 were tested using the national standard GB18445-2012 “Cement-based penetrating crystalline waterproof material”. The results are shown in Table 1.
[0052] Table 1 Waterproof material performance test of Examples 1 to 10 and Comparative Example 1
[0053]
[0054] As shown in Table 1, compared with Comparative Example 1, the impermeability pressure of the embodiment is higher, and the first impermeability pressure of Embodiment 5 and Embodiment 6 can reach up to 1.5Mpa, which is 150% higher than Comparative Example 1, and the second impermeability pressure is up to 1.5MPa, and the impermeability recovery rate is also significantly improved compared with the comparative example. As the core component of the permeable crystallization type concrete waterproof material, the chelating agent can promote cement hydration in cement mortar on the one hand, and accelerate the generation of hydrated calcium silicate gel. On the other hand, it can react with free calcium ions to generate calcium ion complexes, which can effectively improve the anti-penetration ability of cement-based materials, and also has good repair ability for cement-based materials after being penetrated. Waterproofing aids can react quickly with hydration products to generate insoluble crystals (including calcium aluminate, calcium sulfonate and calcium carbonate, etc.), thereby slowing down the water seepage speed in the cracks, reducing the dissolution of hydration products, and improving the generation efficiency of hydrated calcium silicate. Therefore, the waterproofing aid has a significant impact on the first impermeability of cement mortar, but has little impact on the second impermeability recovery rate.
[0055] Cement-based materials with good impermeability often have good compactness and mechanical properties, which are positively correlated. The compressive strength and flexural strength of Example 6 are 59.8MPa and 9.5MPa respectively. The most significant effect on compressive strength is the dosage of active silicon waterproofing agent, which provides SiO32- and AlO3-, increasing the amount of hydrated calcium silicate gel and calcium aluminate crystals in cement mortar, making its structure more compact, and therefore significantly improving the compressive strength of cement mortar.
[0056] Finally, it should be noted that, in this article, words such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of more restrictions, an element defined by the sentence "comprises a ..." does not exclude the presence of other identical elements in the process, method, article or device including the element.
[0057] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0058] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. An airport pavement permeable crystalline concrete waterproof material, characterized in that: It includes at least the following components in parts by weight: 48-52 parts of cement, 15-20 parts of industrial solid waste, 30-35 parts of quartz sand, 0.25-0.75 parts of active silicon waterproofing agent, 0.2-0.4 parts of complexing agent, 0.1-0.3 parts of waterproofing agent, and 0.2-0.6 parts of calcium ion compensator.
2. The airport pavement permeable crystalline concrete waterproof material according to claim 1, characterized in that: It includes at least the following components in parts by weight: 50 parts of cement, 18 parts of industrial solid waste, 30 parts of quartz sand, 0.25 parts of active silicon waterproofing agent, 0.2 parts of complexing agent, 0.1 parts of waterproofing agent, and 0.2 parts of calcium ion compensator.
3. The airport pavement permeable crystalline concrete waterproof material according to claim 1, characterized in that: It includes at least the following components in parts by weight: 50 parts of cement, 18 parts of industrial solid waste, 30 parts of quartz sand, 0.5 parts of active silicon waterproofing agent, 0.2 parts of complexing agent, 0.3 parts of waterproofing agent, and 0.4 parts of calcium ion compensator.
4. The airport pavement permeable crystalline concrete waterproof material according to claim 1, characterized in that: It includes at least the following components in parts by weight: 50 parts of cement, 18 parts of industrial solid waste, 30 parts of quartz sand, 0.75 parts of active silicon waterproofing agent, 0.2 parts of complexing agent, 0.2 parts of waterproofing agent, and 0.6 parts of calcium ion compensator.
5. The airport pavement permeable crystalline concrete waterproof material according to any one of claims 1 to 4, characterized in that: The industrial solid waste includes at least fly ash and slag, the weight ratio of fly ash to slag is 1-2:1, and the relative density of fly ash is 1.9-2.4g / cm 3 , slag is ground to a specific surface area greater than 400m 2 / kg.
6. The airport pavement permeable crystalline concrete waterproof material according to any one of claims 1 to 4, characterized in that: The cement is 42.5 ordinary Portland cement, in which particles with a particle size of less than 5 μm account for 14%-16% of the total weight of the cement; the particle size of the quartz sand is 0.1-0.3 mm, and the mud content is 0.04%.
7. The airport pavement permeable crystalline concrete waterproof material according to any one of claims 1 to 4, characterized in that: The active silicon waterproofing agent is a mixture of sodium methyl silicate and sodium aluminate in a weight ratio of 3:
1.
8. The airport pavement permeable crystalline concrete waterproof material according to any one of claims 1 to 4, characterized in that: The complexing agent is a mixture of glycine and calcium lignin sulfonate in a weight ratio of 2.5:
1.
9. The airport pavement permeable crystalline concrete waterproof material according to any one of claims 1 to 4, characterized in that: The waterproofing auxiliary agent is a mixture of calcined coal gangue and desulfurized gypsum in a weight ratio of 1:1; the calcium ion compensator is steel slag powder.
10. The method for preparing the airport pavement permeable crystalline concrete waterproof material according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: S1. Mix 48-52 parts of cement, 15-20 parts of industrial solid waste and 30-35 parts of quartz sand in a dry powder mixer to obtain a premix A; the mixing time is 4-8 minutes; S2. Add 0.25-0.75 parts of active silicon waterproofing agent, 0.2-0.4 parts of complexing agent, 0.1-0.3 parts of waterproofing agent and 0.2-0.6 parts of calcium ion compensator to the premix A obtained in step S1 in sequence; stir evenly to obtain the airport pavement permeable crystalline concrete waterproof material.