New process for purifying waste polyester alcoholysis product
Through the combination of temperature-controlled reactor and flash evaporator, combined with melt crystallization and thermal filtration technology, the problem of difficult removal of dye impurities in waste polyesters is solved, and the purification of high-purity BHET and the improvement of energy consumption utilization are achieved, which improves the improvement of high-purity BHET Performance of recycled polyester.
Patent Information
- Application Number
- CN202411097813.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, in the recycling process of waste polyester, it is difficult to effectively remove dye impurities in polyester, resulting in impure color and poor shear performance of recycled polyester, which limits the efficient recycling and regeneration of waste polyester.
A new purification process for waste polyester alcohol dissolution products is adopted, and alcohol dissolution is carried out through a temperature-controlled reactor, and then ethylene glycol is removed in the flash evaporator, and polymer impurities are removed by melt crystallization technology, combined with thermal filtration and Refining treatment improves the purity and color quality of BHET.
It realizes high purity purification of BHET, improves energy consumption utilization, significantly reduces the color impurities of the product, and improves the performance of recycled polyester. It is suitable for the raw material production of light-colored low-melting point, high-quality colored polyester staple fibers.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of waste polyester resource utilization technology, and more specifically, it relates to a new process for purifying waste polyester alcoholysis products. Background Technology
[0002] Polyethylene terephthalate (PET), commonly known as polyester, is a high-performance semi-crystalline thermoplastic polymer widely used in chemical fibers, packaging, pharmaceuticals, and electronics. While the polyester industry has experienced rapid growth, PET's inertness, hydrophobicity, and high molecular weight make it resistant to microbial attack and biodegradable, exhibiting strong resistance to degradation in natural environments. As a result, waste polyester is often collected in landfills or scattered in the environment, and a significant portion of improperly recycled polyester ends up in soil and oceans. Against this backdrop, the enormous stockpile of waste polyester products not only places immense pressure on the ecological environment but also represents a serious waste of petrochemical resources.
[0003] Based on the physicochemical properties of polyester, its recycling methods are mainly divided into two types: physical recycling and chemical recycling. Physical recycling, based on the thermoplasticity of polyester, regenerates polyester by removing impurities, washing, crushing, drying, and then melting and regranulating waste polyester products. While physical recycling is low-cost and technically simple, it can only achieve downgraded recycling of polyester, and the number of recycling cycles is limited, failing to achieve a closed-loop cycle. Chemical recycling, based on the reversibility of polyester polycondensation and the nucleophilic mechanism of transesterification, uses small-molecule depolymerizing agents to attack large molecular chains, causing polyester to depolymerize into monomers or intermediates. After separation and purification, these are then repolymerized to achieve regeneration. This method not only achieves efficient resource reuse but also conforms to the principles of environmental sustainability, making it a more ideal recycling method.
[0004] Currently, the industrial recycling of high-purity polyester bottles and light-colored polyester is widely commercialized. However, when polyester is used as a clothing raw material, it is often dyed in the spinning process or later in the yarn production, and may contain a large amount of oil and other impurities after use. After processing and recycling, the product properties of polyester will decrease, limiting the performance of downstream products. Moreover, the shear properties of waste polyester are significantly reduced compared to virgin polyester. The recycled polyester is not pure in color, and its strength and shear properties are worse than those of virgin polymerized polyester products. The color also differs greatly, severely limiting the promotion of waste polyester recycling methods. To further reduce the impact of polyester color on the performance of recycled polyester, the alcoholysis solution of colored waste polyester is decolorized. Although colored dyes coexist with polyester macromolecules during depolymerization, the dyes can be removed from the alcoholysis solution system using certain technologies. In the ethylene glycol alcoholysis process of PET, an excess catalyst is added to catalyze the alcoholysis reaction with ethylene glycol. After depolymerization, unreacted polyester and oligomers generated during depolymerization are removed from the mixture by hot filtration, utilizing the difference in solubility. Excess ethylene glycol is then recovered by vacuum distillation. The recovered ethylene glycol can be reused to depolymerize waste polyester again. In the second stage of the depolymerization process, the polyester is broken down into monomers or small molecules that dissolve in various solvents, such as alcohols, esters, nitriles, chlorinated hydrocarbons, ketones, or water. The reaction solution is thoroughly filtered while hot to remove disperse dyes from the polyester. Solvent displacement allows for a certain degree of removal of disperse dyes. Furthermore, the BHET obtained after alcoholysis of waste polyester contains unsaturated compounds with double bonds, such as aldehydes and ethers, as well as sulfides. These chromophores cause the BHET product after ethylene glycol alcoholysis of waste polyester to retain a certain color, thus increasing the difficulty of PET recycling. Summary of the Invention
[0005] The purpose of this invention is to address the shortcomings of existing technologies by providing a new purification process for waste polyester alcoholysis products that offers high BHET purity, high energy efficiency, and low color impurities.
[0006] To achieve the above technical objectives, the technical solution adopted in the new process for purifying waste polyester alcoholysis products of the present invention is as follows: A novel process for purifying waste polyester alcoholysis products includes the following steps: S1. Chop the waste polyester, weigh the waste polyester, ethylene glycol and catalyst according to the mass ratio, add them to the temperature-controlled reactor, start stirring and purge with nitrogen. Purge with nitrogen until the reactor is slightly positive, release the nitrogen and purge with nitrogen again. Repeat the operation three times. The S2 reactor is heated to 190–220°C, kept at this temperature, and the pressure is controlled at 0.01–1.0 MPa. The reactor is stirred and reacted for 3 hours. After the S3 reaction is completed, the reaction solution is filtered and transferred to a flash evaporator, where most of the ethylene glycol is removed under vacuum. S4 Under the heat preservation condition, the above materials are transferred to the crystallization reactor for melting and crystallization. The stirring speed of the crystallization reactor is controlled at 2-10 rpm, the cooling rate is controlled at less than 1°C per minute, the temperature at the crystallization endpoint is controlled at 105-110°C, and the BHET product and BHET polymer product are obtained by hot filtration. S5 The BHET product from step S4 is further refined to obtain refined BHET. The equation for the alcoholysis-depolymerization reaction in step S2 is: (1) (2) (3).
[0007] Preferably, in step S1, the mass ratio of each component is based on the mass of waste polyester, the amount of ethylene glycol is 0.5 to 10.0% (wt%) of the amount of waste polyester, and the amount of catalyst is 0.1 to 10.0% (wt%) of the amount of waste polyester.
[0008] Preferably, the waste polyester in step S1 is diethylene terephthalate (PET), including bottle flakes, foam, and textiles.
[0009] Preferably, the ethylene glycol in step S1 is industrial-grade ethylene glycol, with a water content and diethylene glycol content of less than 100 ppm.
[0010] Preferably, the catalyst for the alcoholysis reaction in step S1 is zinc acetate or zinc acetate hydrate.
[0011] Compared with the prior art, the beneficial effects of the present invention are: This invention involves heating the alcoholysis reaction, then hot-filtering and flash-evaporating the alcoholysis products to remove ethylene glycol. The molten alcoholysis products are then crystallized, fully utilizing the heat from the alcoholysis heating process to complete the removal of ethylene glycol and molten crystallization, thus improving overall energy efficiency. Furthermore, by exploiting the difference in crystallization properties between the alcoholysis depolymerization product BHET and its polymers, the molten alcoholysis products are gradually cooled to prevent BHET from crystallizing while allowing the polymers to crystallize. Hot filtration is then performed to remove the crystallized polymers, resulting in BHET with higher purity and a superior color compared to the alcoholysis products. Detailed Implementation
[0012] The invention will be further described below with reference to specific embodiments: A novel process for purifying waste polyester alcoholysis products includes the following steps: S1. Chop the waste polyester, weigh the waste polyester, ethylene glycol and catalyst according to the mass ratio, add them to the temperature-controlled reactor, start stirring and purge with nitrogen. Purge with nitrogen until the reactor is slightly positive, release the nitrogen and purge with nitrogen again. Repeat the operation three times. The S2 reactor is heated to 190–220°C, kept at this temperature, and the pressure is controlled at 0.01–1.0 MPa. The reactor is stirred and reacted for 3 hours. After the S3 reaction is completed, the reaction solution is filtered and transferred to a flash evaporator, where most of the ethylene glycol is removed under vacuum. S4 Under the heat preservation condition, the above materials are transferred to the crystallization reactor for melting and crystallization. The stirring speed of the crystallization reactor is controlled at 2-10 rpm, the cooling rate is controlled at less than 1°C per minute, the temperature at the crystallization endpoint is controlled at 105-110°C, and the BHET product and BHET polymer product are obtained by hot filtration. S5 The BHET product from step S4 is further refined to obtain refined BHET. The equation for the alcoholysis-depolymerization reaction in step S2 is: (1) (2) (3).
[0013] In this invention, the mass ratio of each component in step S1 is based on the mass of waste polyester, the amount of ethylene glycol is 0.5 to 10.0% (wt%) of the amount of waste polyester, and the amount of catalyst is 0.1 to 10.0% (wt%) of the amount of waste polyester.
[0014] In this invention, the waste polyester in step S1 is diethylene terephthalate (PET), including bottle flakes, foam materials and textiles, the ethylene glycol is industrial grade ethylene glycol, and its water content and diethylene glycol content are both less than 100 ppm. The catalyst for the alcoholysis reaction is zinc acetate or zinc acetate hydrate.
[0015] In this invention, after the depolymerization reaction of waste polyester ethylene glycol is completed, some impurities are removed by filtration, and unreacted ethylene glycol is removed by flash evaporation. Then, the alcoholysis product in the molten state after the removal of ethylene glycol is crystallized to further remove impurities. Finally, the "sweat" product is heated and melted to form granules, which can be used as raw materials for light-colored, low-melting-point, high-quality colored polyester staple fibers. At the same time, the heat from alcoholysis heating is fully utilized to complete the removal of ethylene glycol and melt crystallization, thereby improving the overall energy consumption efficiency.
[0016] Preparation Example In a 1000mL stirred reactor, 300g of ethylene glycol and 6g of catalyst were added sequentially. The mixture was heated to 100℃ and stirred for 30 minutes to dissolve. Then, 60g of waste polyester (dark military uniform material) was added. The mixture was stirred and the temperature was controlled between 195℃±2℃. At this time, the reaction pressure was 0.05MPa±0.01MPa. After reacting for 3 hours, the mixture was filtered while hot. The filtrate was transferred to a flash evaporator under heat preservation and most of the ethylene glycol was removed under vacuum. The mixture was then transferred to a crystallization reactor under heat preservation for melt crystallization. The crystallization temperature was strictly controlled and the mixture was filtered while hot to obtain crude BHET product and BHET polymer product.
[0017] The crude BHET product also contains a small amount of ethylene glycol. Adding the crude BHET product to hot water forms a homogeneous aqueous solution, followed by cooling and crystallization. After filtration, the refined BHET product can be obtained. The BHET polymer product also contains a small amount of ethylene glycol. After cooling, it becomes a solid and can be used as an "esterified product" to synthesize different low-melting-point polyester products with special polyester monomers.
[0018] The BHET content of the crude BHET product was determined using liquid chromatography, and the color of the sample was measured using a colorimeter. At this point, the alcoholysis conversion rate of the fabric was close to 100% (no insoluble matter was observed after filtration of the alcoholysis liquid), the BHET selectivity was greater than 80%, the ratio of crude BHET product to BHET polymer product was 4-5:1, and the color B values of the crude BHET product and the BHET polymer product were less than 3 and greater than 5, respectively.
[0019] Example 1 In a 1000mL stirred reactor, 300g of ethylene glycol and 6g of catalyst were added sequentially. The mixture was heated to 100℃ and stirred for 30 minutes to dissolve. Then, 60g of waste polyester (dark-colored military uniform material) was added. Stirring was maintained, and the temperature was controlled between 195℃±2℃. The reaction pressure was 0.05MPa±0.01MPa. After reacting for 3 hours, the mixture was filtered while hot. Under the condition of heat preservation, the filtrate was transferred to a flash evaporator, and 150g of ethylene glycol was removed under vacuum. Under the condition of heat preservation, the above materials were transferred to a crystallization reactor for melt crystallization. The crystallization temperature was strictly controlled at 110℃, and the mixture was filtered while hot to obtain crude BHET product and BHET polymer product.
[0020] At this point, the ratio of crude BHET product to BHET polymer product is 4.5:1, and the color B values of crude BHET product and BHET polymer product are 2.6 and greater than 5.7, respectively.
[0021] Example 2 In a 1000mL stirred reactor, 300g of ethylene glycol and 6g of catalyst were added sequentially. The mixture was heated to 100℃ and stirred for 30 minutes to dissolve. Then, 60g of waste polyester (dark military uniform material) was added. The mixture was stirred and the temperature was controlled between 195℃±2℃. The reaction pressure was 0.05MPa±0.01MPa. After reacting for 3 hours, the mixture was filtered while hot. The filtrate was transferred to a flash evaporator under heat preservation and 180g of ethylene glycol was removed under vacuum. The mixture was then transferred to a crystallization reactor under heat preservation for melt crystallization. The crystallization temperature was strictly controlled at 110℃. The mixture was then filtered while hot to obtain crude BHET product and BHET polymer product.
[0022] At this point, the ratio of crude BHET product to BHET polymer product is 4.2:1, and the color B values of crude BHET product and BHET polymer product are 2.4 and greater than 5.5, respectively.
[0023] Example 3 In a 1000mL stirred reactor, 300g of ethylene glycol and 6g of catalyst were added sequentially. The mixture was heated to 100℃ and stirred for 30 minutes to dissolve. Then, 60g of waste polyester (dark military uniform material) was added. The mixture was stirred and the temperature was controlled between 195℃±2℃. The reaction pressure was 0.05MPa±0.01MPa. After reacting for 3 hours, the mixture was filtered while hot. The filtrate was transferred to a flash evaporator under heat preservation and 210g of ethylene glycol was removed under vacuum. The mixture was then transferred to a crystallization reactor under heat preservation for melt crystallization. The crystallization temperature was strictly controlled at 110℃. The mixture was then filtered while hot to obtain crude BHET product and BHET polymer product.
[0024] At this point, the ratio of crude BHET product to BHET polymer product is 4.0:1, and the color B values of crude BHET product and BHET polymer product are 2.3 and greater than 5.3, respectively.
[0025] Example 4 In a 1000mL stirred reactor, 300g of ethylene glycol and 6g of catalyst were added sequentially. The mixture was heated to 100℃ and stirred for 30 minutes to dissolve. Then, 60g of waste polyester (dark military uniform material) was added. The mixture was stirred and the temperature was controlled between 195℃±2℃. The reaction pressure was 0.05MPa±0.01MPa. After reacting for 3 hours, the mixture was filtered while hot. The filtrate was transferred to a flash evaporator under heat preservation and 180g of ethylene glycol was removed under vacuum. The mixture was then transferred to a crystallization reactor under heat preservation for melt crystallization. The crystallization temperature was strictly controlled at 105℃. The mixture was filtered while hot to obtain crude BHET product and BHET polymer product.
[0026] At this point, the ratio of crude BHET product to BHET polymer product is 4.3:1, and the color B values of crude BHET product and BHET polymer product are 2.5 and greater than 5.3, respectively.
[0027] In summary, these are merely preferred embodiments of the present invention and are not intended to limit the scope of the invention. All equivalent variations and modifications made in accordance with the shape, structure, features, and spirit of the claims of the present invention should be included within the scope of the claims of the present invention.
Claims
1. A new process for purifying waste polyester alcoholysis products, characterized in that: The following steps are involved: S1 Chop the waste polyester into pieces, weigh the waste polyester, ethylene glycol and catalyst according to the mass ratio, add them into a temperature-controlled reactor, start stirring and introduce nitrogen replacement. Nitrogen replacement is to introduce nitrogen to the reactor until the pressure is slightly positive, release nitrogen and then introduce nitrogen, and repeat the operation three times; S2 The reactor was heated to 190-220°C, kept warm and the pressure was controlled at 0.01-1.0 MPa, and stirred for 3 hours; After the reaction in S3 is completed, the reaction solution is filtered and transferred to a flash evaporator to remove most of the ethylene glycol under vacuum; S4. Under the heat preservation state, the above materials are transferred to a crystallization reactor for melt crystallization, the stirring speed of the crystallization reactor is controlled at 2-10 rpm, the cooling rate is controlled to be less than 1°C per minute, the temperature at the crystallization end point is controlled to be 105-110°C, and the BHET product and BHET polymer product are obtained by hot filtration; S5: The BHET product in step S4 is further refined to obtain refined grade BHET; The alcoholysis depolymerization reaction equation in step S2 is: (1) (2) (3)。 2. The new process for purifying waste polyester alcoholysis products according to claim 1, characterized in that: The mass ratio of each component in step S1 is based on the mass of the waste polyester, the amount of ethylene glycol used is 0.5-10.0% (wt%) of the waste polyester used, and the amount of catalyst used is 0.1-10.0% (wt%) of the waste polyester used.
3. The new process for purifying waste polyester alcoholysis products according to claim 1, characterized in that: The waste polyester in step S1 is diethylene glycol terephthalate (PET), including bottle flakes, foam materials and textiles.
4. The new process for purifying waste polyester alcoholysis products according to claim 1, characterized in that: The ethylene glycol in step S1 is industrial grade ethylene glycol, and its water content and diethylene glycol content are both less than 100 ppm.
5. The new process for purifying waste polyester alcoholysis products according to claim 1, characterized in that: The alcoholysis reaction catalyst in step S1 is zinc acetate or hydrated zinc acetate.
Citation Information
Cited By
Polyester flash non-woven fabric and preparation method thereof
CN119465518A
Method for realizing high-purity and high-yield preparation of BHET (butylated hydroxytoluene) by depolymerizing waste PET (polyethylene terephthalate)
CN120483880A
A method for depolymerizing waste PET to achieve high-purity and high-yield preparation of BHET
CN120483880B
Chain extender based on waste PET, polyurethane sponge and preparation method
CN121248417A
Process device for preparing BHET polymer powder from waste polyester and buffer storage bin
CN122625473A