Solution polymerized styrene-butadiene rubber for polymer modification and preparation method thereof
By combining a novel polar furan-based structure modifier with a traditional modifier, the synthesis problem of random copolymer styrene-butadiene rubber in anionic polymerization was solved, achieving a highly efficient polymer modification and toughening effect.
Patent Information
- Application Number
- CN202411143126.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-01
AI Technical Summary
Existing technologies make it difficult to synthesize random copolymerized styrene-butadiene rubber via anionic polymerization, which limits its application as a toughness and impact modifier in polymer modification.
A novel polar furan-based structure modifier was combined with a traditional structure modifier to form a binary modifier system. This system, along with an organolithium initiator and a cyclohexane solvent, was used to synthesize solution-polymerized styrene-butadiene rubber, thereby modulating the copolymerization reaction of styrene and butadiene.
Solution-polymerized styrene-butadiene rubber with a balance between the content of functional groups and the degree of randomization was prepared, which significantly improved the toughening effect in polymer modification and was superior to single modifiers and commercially available rubbers.
Smart Images

Figure BDA0005001482890000021 
Figure BDA0005001482890000031 
Figure BDA0005001482890000061
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer technology, and specifically discloses a solution-polymerized styrene-butadiene rubber for polymer modification and a preparation method thereof. Background Art
[0002] Solution-polymerized styrene butadiene rubber is an anionic random polymer formed by the initiation of styrene and butadiene monomers in hydrocarbon solvents under the action of organic lithium. Compared with other types of rubber, its synthetic reaction system is in solution, and the polymerization process is anionic polymerization. Solution-polymerized styrene butadiene rubber has developed rapidly as a precursor material for mid-to-high-end tires, but the solution-polymerized styrene butadiene rubber used as a toughness and impact modifier in polymer modification has fewer brands than the former and has long been monopolized by foreign countries. With the continuous expansion of domestic production of polymers such as ABS and HIPS, my country's demand for solution-polymerized styrene butadiene rubber will inevitably increase significantly in the future. Therefore, the research and development of high-quality solution-polymerized styrene butadiene rubber for polymer modification has become a domestic concern and urgent issue to be solved.
[0003] In industrial production, the production process of random solution-polymerized styrene butadiene rubber mainly includes five parts: raw material refining, initiator preparation, copolymerization, solvent recovery and rubber post-treatment. At present, the mainstream synthesis method of solution-polymerized styrene butadiene rubber uses cyclohexane as solvent, organic lithium as initiator, and microstructure regulation by binary regulator. However, during the synthesis process, when ensuring that the 1,2-vinyl content in the product is relatively ideal, due to the large difference in the reactivity ratio of butadiene and styrene, it is difficult to obtain random copolymerized styrene butadiene rubber, which makes it impossible to use it as a toughness and impact modifier in polymer modification.
[0004] Therefore, it is necessary to develop a solution-polymerized styrene-butadiene rubber and a preparation method thereof for polymer modification in order to solve the above-mentioned technical problems. Summary of the invention
[0005] The technical solution adopted by the present invention is as follows:
[0006] In a first aspect, the present invention provides a method for preparing a polymer-modified solution-polymerized styrene-butadiene rubber, which specifically comprises the following steps:
[0007] S1 Preparation of binary regulating system: The new polar furan structure regulator and the traditional structure regulator are compounded in a mass ratio of 7:3 to 3:2 to form a binary regulating system;
[0008] The preparation of the novel polar furan structure regulator comprises the following steps:
[0009] (1) 20-30 parts by weight of acetone, 50-75 parts by weight of a furan compound, and 1-5 parts by weight of a strong acid solution are thoroughly mixed and reacted at 40-60° C. to obtain a mixture;
[0010] (2) adding a strong base and a weak acid salt solution dropwise to the mixture obtained in step (1) and mixing thoroughly until the solution becomes neutral;
[0011] (3) extracting the product obtained in step (2) with an ester organic matter and washing with deionized water;
[0012] (4) drying the substance obtained in step (3) with anhydrous sulfate, filtering and then distilling under reduced pressure to obtain an intermediate product A;
[0013] (5) adding 100-200 parts by weight of methanol as a solvent to a reaction kettle, and sequentially adding 30-60 parts by weight of the intermediate product A and 0.1-0.5 parts by weight of a catalyst, reacting at 130-160° C. for 3-6 hours in a hydrogen atmosphere, and then performing reduced pressure distillation to obtain a novel polar furan structure regulator;
[0014] The furan compound is one or a mixture of two or more of 2-methylfuran, tetrahydrofuran, and 2-methyltetrahydrofuran;
[0015] The strong acid solution is one of a 30-60% sulfuric acid solution or a 15-30% hydrochloric acid solution;
[0016] The strong base and weak acid salt is one of carbonate and bicarbonate;
[0017] The catalyst is one of diphenylphosphinocene palladium dichloride, tetrakistriphenylphosphine palladium, dichlorobistriphenylphosphine palladium, and palladium on carbon;
[0018] S2 solution polymerized styrene butadiene rubber synthesis: using organic lithium as initiator, cyclohexane as solvent, styrene and butadiene as raw materials, solution polymerized styrene butadiene rubber is synthesized under the action of a binary composite structure regulator.
[0019] Preferably, the traditional structure regulator is one or a mixture of two or more of tetrahydrofuran, tetrahydrofurfuryl ether, sodium dodecylbenzene sulfonate, pentamethyldiethyltriamine.
[0020] Preferably, in step S2, the raw materials are composed of the following mass fractions:
[0021]
[0022]
[0023] Furthermore, the organic lithium is one of n-butyl lithium, isopropyl lithium, pentyl lithium, sec-butyl lithium, ethyl lithium and propyl lithium.
[0024] Furthermore, the molar ratio of the structure regulator to the organic lithium is controlled at (2-7):1.
[0025] Furthermore, the method for preparing the solution-polymerized styrene-butadiene rubber described in S2 is characterized by comprising the following steps:
[0026] Cyclohexane, styrene and butadiene are added into a reactor, and then a binary composite structure regulator is added, and the mixture is kept in a constant temperature water bath at 60-80°C for 0.5-2h; an initiator organic lithium is added into the reactor according to the designed amount for polymerization reaction, and the styrene / butadiene copolymerization temperature is set at 60-80°C for polymerization reaction; isopropanol is added into the reactor to terminate the polymerization reaction, and a solution-polymerized styrene-butadiene rubber is obtained.
[0027] In a second aspect, the present invention provides a solution-polymerized styrene-butadiene rubber prepared by the method described in the first aspect.
[0028] In a third aspect, the present invention provides a use of the solution-polymerized styrene-butadiene rubber described in the second aspect for preparing ABS.
[0029] Preferably, the application of the solution polymerized styrene-butadiene rubber for the preparation of ABS comprises the following steps:
[0030] The solution polymerized styrene-butadiene rubber and rubber are fully dissolved in styrene, and then acrylonitrile and ethylbenzene are added, and an initiator and a chain transfer agent are added dropwise. After being fully stirred, ABS is synthesized at 100-150°C.
[0031] Furthermore, the added amount of the solution-polymerized styrene-butadiene rubber is 1-5%.
[0032] In a fourth aspect, the present invention provides a novel polar furan structure regulator, the preparation of which comprises the following steps:
[0033] (1) 20-30 parts by weight of acetone, 50-75 parts by weight of a furan compound, and 1-5 parts by weight of a strong acid solution are thoroughly mixed and reacted at 40-60° C. to obtain a mixture;
[0034] (2) adding a strong base and a weak acid salt solution dropwise to the mixture obtained in step (1) and mixing thoroughly until the solution becomes neutral;
[0035] (3) extracting the product obtained in step (2) with an ester organic matter and washing with deionized water;
[0036] (4) drying the substance obtained in step (3) with anhydrous sulfate, filtering and then distilling under reduced pressure to obtain an intermediate product A;
[0037] (5) adding 100-200 parts of methanol as a solvent to a reaction kettle, and sequentially adding the intermediate product A and 0.1-0.5 parts of a catalyst, reacting at 130-160° C. for 3-6 hours in a hydrogen atmosphere, and then performing reduced pressure distillation to obtain a novel polar furan structure regulator;
[0038] The furan compound is one or a mixture of two or more of 2-methylfuran, tetrahydrofuran, and 2-methyltetrahydrofuran;
[0039] The strong acid solution is one of a 30-60% sulfuric acid solution or a 15-30% hydrochloric acid solution;
[0040] The saturated strong base and weak acid salt is one of saturated carbonate or bicarbonate solutions;
[0041] The catalyst is one of diphenylphosphinocene palladium dichloride, tetrakistriphenylphosphine palladium, dichlorobistriphenylphosphine palladium, and palladium on carbon.
[0042] Beneficial effects achieved by the present invention:
[0043] The present invention develops a regulator and compounds it with another existing regulator. The two regulators play a synergistic role in the synthesis of solution-polymerized styrene-butadiene rubber, so as to prepare a solution-polymerized styrene-butadiene rubber capable of balancing the content of functional groups and the degree of randomization. After the solution-polymerized styrene-butadiene rubber is used for small-scale toughening modification of bulk ABS resin, compared with rubber synthesized by a single regulator and some existing rubbers on the market, the toughening effect is more obvious and the influence on other properties is less. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the following examples. It should be noted that the present invention is not limited to the following examples.
[0045] Example 1
[0046] Weigh 27 parts of acetone, 70 parts of 2-methylfuran, and 3 parts of 50% sulfuric acid solution in a round-bottom flask and mix thoroughly, control the reaction temperature to 50°C for 12 hours, then drop saturated sodium bicarbonate solution into the mixture and mix thoroughly until the pH of the solution is 7; extract the obtained mixture with 70 parts of ethyl acetate, wash with deionized water, and then fully dry with anhydrous magnesium sulfate, filter and perform vacuum distillation to obtain intermediate product A. Add 150 parts of methanol to the reactor, and add 50 parts of intermediate product A and 0.2 parts of catalyst palladium carbon in sequence, react at 150°C in a hydrogen atmosphere for 5 hours, and then perform vacuum distillation to obtain a novel polar furan structure regulator.
[0047] Weigh 70 parts of the novel polar furan structure regulator and 30 parts of sodium dodecylbenzene sulfonate and mix the two raw materials thoroughly to form a binary composite structure regulator.
[0048] 90 parts of dried cyclohexane, 3 parts of purified styrene and 7 parts of purified butadiene were added to the reactor, and then 0.1 parts of binary composite structure regulator were added, and the mixture was kept in a constant temperature water bath at 70°C for 1 hour, and then 0.01 parts of n-butyl lithium were used to break the impurities, and then 0.03 parts of initiator n-butyl lithium were added to the reactor for polymerization reaction, and the styrene / butadiene copolymerization temperature was set to 70°C, and the polymerization reaction time was 2 hours. Finally, isopropanol was added to the reactor to terminate the reaction, and solution-polymerized styrene-butadiene rubber was obtained after post-treatment.
[0049] Take 4 parts of homemade solution-polymerized styrene-butadiene rubber and 4 parts of commercially available 97C rubber, place them in 74 parts of styrene and fully dissolve them, then add 18 parts of acrylonitrile and 20 parts of ethylbenzene, drop 0.015 parts of initiator 1,1-(di-tert-butyl peroxide) cyclohexane and 0.12 parts of chain transfer agent n-dodecyl mercaptan, stir well and add to the pilot reactor. The reaction is carried out in three stages, each lasting 2 hours, and the reaction temperatures of each stage are 115°C, 130°C, and 145°C, respectively. After the reaction is completed, the material is devolatilized to obtain a pilot ABS resin.
[0050] Example 2
[0051] Keeping the other steps in Example 1 unchanged, the binary composite structure regulator is replaced with a homemade new polar furan structure regulator.
[0052] Example 3
[0053] Keeping other steps in Example 1 unchanged, the binary composite structure regulator is replaced with a single structure regulator sodium dodecylbenzene sulfonate.
[0054] Example 4
[0055] The commercially available solution polymerized butadiene styrene rubber S1322 was directly used to replace the homemade solution polymerized butadiene styrene rubber in Example 1. The ABS resin polymerization step was the same as that in Example 1.
[0056] Test results
[0057] Table 1 Example test results
[0058]
[0059]
[0060] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a polymer-modified solution-polymerized styrene-butadiene rubber, characterized in that: The specific steps include: S1 Preparation of binary regulating system: The new polar furan structure regulator and the traditional structure regulator are compounded in a mass ratio of 7:3 to 3:2 to form a binary regulating system; The preparation of the novel polar furan structure regulator comprises the following steps: (1) 20-30 parts by weight of acetone, 50-75 parts by weight of a furan compound, and 1-5 parts by weight of a strong acid solution are thoroughly mixed and reacted at 40-60° C. to obtain a mixture; (2) adding a strong base and a weak acid salt solution dropwise to the mixture obtained in step (1) and mixing thoroughly until the solution becomes neutral; (3) extracting the product obtained in step (2) with an ester organic matter and washing with deionized water; (4) drying the substance obtained in step (3) with anhydrous sulfate, filtering and then distilling under reduced pressure to obtain an intermediate product A; (5) adding 100-200 parts by weight of methanol as a solvent to a reaction kettle, and sequentially adding 30-60 parts by weight of the intermediate product A and 0.1-0.5 parts by weight of a catalyst, reacting at 130-160° C. in a hydrogen atmosphere, and then performing reduced pressure distillation to obtain a novel polar furan structure regulator; The furan compound is one or a mixture of two or more of 2-methylfuran, tetrahydrofuran, and 2-methyltetrahydrofuran; The strong acid solution is one of a 30-60% sulfuric acid solution or a 15-30% hydrochloric acid solution; The strong base and weak acid salt is one of carbonate and bicarbonate; The catalyst is one of diphenylphosphinocene palladium dichloride, tetrakistriphenylphosphine palladium, dichlorobistriphenylphosphine palladium, and palladium on carbon; S2 solution polymerized styrene butadiene rubber synthesis: using organic lithium as initiator, cyclohexane as solvent, styrene and butadiene as raw materials, solution polymerized styrene butadiene rubber is synthesized under the action of a binary composite structure regulator.
2. The method for preparing a polymer-modified solution-polymerized styrene-butadiene rubber according to claim 1, characterized in that: The conventional structure regulator is one or a mixture of two or more of tetrahydrofuran, tetrahydrofurfuryl ether, sodium dodecylbenzene sulfonate and pentamethyldiethyltriamine.
3. The method for preparing a polymer-modified solution-polymerized styrene-butadiene rubber according to claim 1, characterized in that: In step S2, the raw materials are composed of the following parts by mass:
4. The method for preparing a polymer-modified solution-polymerized styrene-butadiene rubber according to claim 3, characterized in that: The organic lithium is one of n-butyl lithium, isopropyl lithium, pentyl lithium, sec-butyl lithium, ethyl lithium and propyl lithium.
5. The method for preparing polymer-modified solution-polymerized styrene-butadiene rubber according to claim 3, characterized in that: The molar ratio of the structure regulator to the organic lithium is controlled at (2-7):
1.
6. The method for preparing a polymer-modified solution-polymerized styrene-butadiene rubber according to claim 1, characterized in that: The method for preparing the solution-polymerized styrene-butadiene rubber described in S2 is characterized by comprising the following steps: Cyclohexane, styrene and butadiene are added into a reactor, and then a binary composite structure regulator is added, and the mixture is kept in a constant temperature water bath at 60-80°C for 0.5-2h; an initiator organic lithium is added into the reactor according to the designed amount for polymerization reaction, and the styrene / butadiene copolymerization temperature is set at 60-80°C for polymerization reaction; isopropanol is added into the reactor to terminate the polymerization reaction, and a solution-polymerized styrene-butadiene rubber is obtained.
7. A solution-polymerized styrene-butadiene rubber prepared by the method according to any one of claims 1 to 6.
8. Use of the solution polymerized styrene-butadiene rubber according to claim 7 in the preparation of ABS.
9. The use of the solution polymerized styrene-butadiene rubber for preparing ABS according to claim 8, characterized in that: The application of the solution polymerized styrene-butadiene rubber for ABS preparation comprises the following steps: The solution polymerized styrene butadiene rubber and rubber are fully dissolved in styrene, then acrylonitrile and ethylbenzene are added, an initiator and a chain transfer agent are added dropwise, and after being fully stirred, ABS is synthesized at 100-150° C. The addition amount of the solution polymerized styrene butadiene rubber is 1-5%.
10. A novel polar furan structure regulator, characterized in that: The preparation comprises the following steps: (1) 20-30 parts by weight of acetone, 50-75 parts by weight of a furan compound, and 1-5 parts by weight of a strong acid solution are thoroughly mixed and reacted at 40-60° C. to obtain a mixture; (2) adding a strong base and a weak acid salt solution dropwise to the mixture obtained in step (1) and mixing thoroughly until the solution becomes neutral; (3) extracting the product obtained in step (2) with an ester organic matter and washing with deionized water; (4) drying the substance obtained in step (3) with anhydrous sulfate, filtering and then distilling under reduced pressure to obtain an intermediate product A; (5) adding 100-200 parts of methanol as a solvent to a reaction kettle, and sequentially adding the intermediate product A and 0.1-0.5 parts of a catalyst, reacting at 130-160° C. in a hydrogen atmosphere, and then performing reduced pressure distillation to obtain a novel polar furan structure regulator; The furan compound is one or a mixture of two or more of 2-methylfuran, tetrahydrofuran, and 2-methyltetrahydrofuran; The strong acid solution is one of a 30-60% sulfuric acid solution or a 15-30% hydrochloric acid solution; The saturated strong base and weak acid salt is one of saturated carbonate or bicarbonate solutions; The catalyst is one of diphenylphosphinocene palladium dichloride, tetrakistriphenylphosphine palladium, dichlorobistriphenylphosphine palladium, and palladium on carbon.
Citation Information
Cited By
Copolymerization modified solution polymerized styrene-butadiene rubber and preparation method thereof
CN120842485A