Low-odor environment-friendly German-standard 105 DEG C low-voltage automobile wire PVC insulating material and preparation method thereof
By using a specific ratio of low-odor and environmentally friendly formula and process treatment in PVC insulating materials, the odor and performance problems in PVC insulating materials for 105℃ low-voltage automobile lines have been solved, and the odor grade and performance improvement has been achieved, meeting the German standard. Require.
Patent Information
- Application Number
- CN202411120593.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to achieve low odor in PVC insulating materials for low-voltage automotive lines at 105°C, and the German standard has higher requirements for long-term aging performance and scratching performance, but the existing methods cannot meet these standards.
Using low-odor, environmentally friendly PVC insulating material formula, including PVC resin, calcium and zinc stabilizer, trioctyl trimelite, porous ceramic adsorbent, lubricants, antioxidants and mineral fillers, processed through specific ratios and processes , improves odor adsorption capacity and material properties.
The odor level of the automobile line reaches ≤3, meets the requirements of the German standard 105℃ low-voltage automobile line, and improves the aging performance and scratching performance of the material.
Smart Images

Figure CN118879005A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an insulating material for electric wires and cables, in particular to a low-odor, environment-friendly German standard 105°C low-voltage PVC insulating material for automotive wires and a preparation method thereof. Background Art
[0002] With the rise of domestic new energy forces, domestic automobile brands pay more attention to product driving quality and in-car safety than joint venture automobile brands and imported cars. In particular, the interior air quality of cars is increasingly valued by domestic automobile brands, and the odor level in the car has become an important reference indicator for evaluating car quality.
[0003] The main sources of odor in automobiles are automobile interiors and their leather, automobile wiring harnesses, and sealing accessories. Among them, the low-voltage wiring harness insulation material in automobile wiring harnesses is PVC insulation material. The PVC resin and plasticizer in the PVC insulation material formula are important sources of odor. The automobile wiring odor level evaluation standard is divided into 1 to 6 levels. If there is a situation between two evaluation levels, a half-level evaluation is allowed. The evaluation standards are as follows:
[0004] Odor level Judging basis Level 1 No odor Level 2 Slight odor, but not disturbing Level 3 There is a noticeable smell, but no disturbing smell Level 4 Disturbing odor Level 5 Has a strong, disturbing odor Level 6 There is an unbearable smell
[0005] The main sources of odor in cable PVC insulation are alcohols and aldehydes in plasticizers, small molecules in stabilizers, and HCl removed from PVC molecular chains. Some research has been done to remove the odor from the above sources.
[0006] Chinese patent CN111040338B discloses a low-odor soft PVC material, which is premixed with large-surface-area nano-calcium carbonate and zinc ricinoleate in a ratio of 3-6.5:3-6.5, and then added to the PVC formula. The principle of this method is that when zinc ricinoleate encounters water or moisture, the activated zinc atoms in zinc ricinoleate can form strong hydrogen bonds with nitrogen and sulfur atoms in the odor. Zinc ricinoleate can also absorb odorous chemical structures, such as amines, ammonia, acids, etc. However, when produced according to the patented method, the deodorization effect is not obvious, mainly because the PVC cable material lacks water and moisture to form hydrogen bonds, and the deodorization effect is not obvious.
[0007] Chinese patent CN109467844B discloses low-odor PVC granules and a preparation method thereof, which uses coconut shell activated carbon and nanoporous aerogel. The production process of the deodorant produced according to this method is complicated, and the deodorant has a cycle of adsorption and desorption, and in the sealed odor test at 80°C × 2h, the odor desorption is obvious and the odor is strong.
[0008] Chinese patent application CN107400317A discloses a low-odor PVC automotive wiring harness material and a preparation method thereof. The method uses porous alumina and activated carbon in combination with plasticizers DINCH, TOTM, DOTP, and DOS. The method belongs to a conventional physical adsorption process, and plasticizers DOTP, DINCH, TOTM, etc. have a strong pungent odor at high temperatures. Experiments conducted according to the patent scheme have no obvious effect and the odor is highly irritating.
[0009] At present, there are no corresponding national and industry standards for the odor level and TVOC test of automotive wiring harnesses in domestic automobile enterprises. All automobile enterprises test according to internal test methods, among which BYD is the most strict. Without any pre-treatment, PVC insulation materials for 105℃ low-voltage automotive wires cannot meet the requirements of BYD Q / BYDQ-A1901.404-2018 "Automotive Parts Odor Test Method" automotive wire odor level test ≤3 level.
[0010] Compared with Japanese standard automotive cables, German standard automotive cables have higher requirements for long-term aging performance, abrasion resistance, etc. German standard automotive cables are required to meet the 3000h aging performance of the corresponding temperature level and the abrasion resistance requirements of the corresponding specification cables, while Japanese standard automotive cables have no relevant requirements. Summary of the invention
[0011] In order to solve the above problems existing in the prior art, the present invention provides a low-odor, environmentally friendly German standard 105°C low-voltage PVC insulating material for automotive wires and a preparation method thereof.
[0012] The PVC insulating material of the invention is studied from aspects of plasticizer, deodorant, stabilizer, etc., so as to achieve the requirement that the odor of the automobile 105°C low-voltage automobile wire using the insulating material is ≤ level 3.
[0013] A low-odor, environmentally friendly German standard 105°C low-voltage automotive wire PVC insulation material, comprising the following raw material components by weight ratio:
[0014] PVC resin: 100 parts,
[0015] Calcium zinc stabilizer: 5-12 parts,
[0016] Trioctyl trimellitate (TOTM): 30-70 parts,
[0017] Porous ceramic adsorbent: 2 to 6 parts,
[0018] Lubricant: 0.4-1.6 parts,
[0019] Antioxidant: 0.4-1.6 parts,
[0020] Acrylate processing aid: 1 to 3 parts,
[0021] Mineral filler: 20-60 parts;
[0022] in:
[0023] The polymerization degree of the PVC resin is 1250-1350, the number of impurity particles is ≤20, and the number of "fish eyes" is ≤15 / 400cm 2 , water extract conductivity ≤ 5 S 2 cm 1 ;
[0024] The requirement for the calcium zinc stabilizer is that the total carbon release at 120°C×4h is ≤100μg·C / g;
[0025] The requirements of the trioctyl trimellitate product include: ester content ≥99.5%, 2-ethylhexanol content ≤100 mg / kg, di(2-ethylhexyl) phthalate content ≤50 mg / kg and dioctyl terephthalate ≤0.6%.
[0026] The microstructure of the porous ceramic adsorbent is a regular pipeline structure, the pipeline diameter is nanometer-level, the pipeline is a spatial network structure, and a surfactant with affinity to VOC is attached in the pipeline.
[0027] The porous ceramic adsorbent is a ceramic powder (such as alumina, zirconium oxide, silicon carbide, etc.) Figure 2 The nanostructured ceramics are composed of a structural template, during which additives (such as binders, enhancers, antioxidants, etc.) can also be further used. The nanotube diameter structure of the template is ≤1nm, and the template pipeline forms a spatial network structure. The ceramic powder is melted in an aqueous solution under high temperature and high pressure, and injected into the nano-template. The pressure, temperature and time are controlled during the molding process to ensure the density and strength of the ceramic. After molding in the template, the template, gouache and other impurities are removed by high-temperature calcination to obtain a primary porous calcined ceramic. Under the action of ion exchange, the porous ceramic will adsorb a layer of surfactant with affinity to VOC inside. After the adsorption is completed, it is dried at 180°C to obtain the final product. First, the pores of the porous ceramics are controlled at about 1nm. In terms of the spatial structure size, the difficulty of odorous VOCs to escape after entering the pore structure increases. Second, the surfactant in the pore structure reduces the binding force between the ceramic and the organic odor VOC molecules, accelerating the adsorption rate and the difficulty of escape at high temperature. Therefore, the adsorbent at low addition can help solve the problems of low adsorption rate and easy desorption at high temperature of conventional adsorbents.
[0028] The method for selecting surfactants that are compatible with VOCs is as follows: for aromatic hydrocarbons in VOCs, such as toluene and xylene, Tween series surfactants can be preferred, and for alcohol VOCs, ionic surfactants are more effective, such as sodium dodecyl sulfate. In automotive wire materials, the sources of odor and VOCs are aromatic hydrocarbons and alcohols. Therefore, preferably, both Tween series surfactants and ionic surfactants are contained.
[0029] The lubricant comprises: polyethylene wax: 0.2-0.8 parts and calcium stearate: 0.2-0.8 parts.
[0030] Both polyethylene wax and calcium stearate can spread and wet the metal surface to form a lubricating layer. The flame-retardant PVC melt is in direct contact with the metal surface. Using them alone can also produce effective metal lubrication.
[0031] Relatively speaking, since the polar head of calcium stearate has a stronger mutual attraction with the metal surface and the interface stability is high, it can effectively resist the mechanical stripping effect of the dynamic PVC melt. Therefore, the metal lubricity of calcium stearate is stronger. Since the polyethylene wax molecules are inserted into the non-polar tail-non-polar tail interface of the calcium stearate lubricating layer and the non-polar tail-PVC melt interface of the calcium stearate lubricating layer to form a slip layer, and the calcium stearate is dispersed into reverse micelles, a slip layer is formed between the calcium stearate reverse micelles-reverse micelles and the calcium stearate reverse micelles-PVC melt, which can reduce the friction between the internal part of the calcium stearate layer adhering to the metal surface and the PVC melt, thereby reducing the destructive effect of the dynamic PVC melt on the lubricating layer and enhancing the ability of the lubricating layer to hinder the direct contact between the PVC melt and the metal surface;
[0032] Calcium stearate dissolves in polyethylene wax and adsorbs on the polyethylene wax-metal interface and polyethylene wax-PVC melt interface, which can enhance the interfacial bonding force, reduce interfacial tension, and improve interfacial stability. It also enhances the ability of the lubricating layer to prevent the direct contact between the PVC melt and the metal surface. Therefore, the interaction between polyethylene wax and calcium stearate can effectively improve the metal lubrication performance and produce an effective coordination effect.
[0033] The antioxidant includes hindered phenol antioxidant and phosphite antioxidant. Specifically, 0.2 to 0.8 parts of antioxidant 1010 and 0.2 to 0.8 parts of antioxidant 168 can be selected.
[0034] During processing and use, PVC materials are susceptible to oxidation and degradation due to factors such as heat, oxygen, and light. Antioxidant 1010 belongs to the hindered phenol antioxidant class. The phenolic hydroxyl group in antioxidant 1010 can react with the free radicals produced by PVC oxidation, providing hydrogen atoms to terminate the free radical chain reaction, thereby inhibiting further oxidation. Secondly, antioxidant 1010 can slow down the oxidation process by capturing peroxyl radicals and reduce the attack of peroxyl radicals on the chain of PVC molecules. Antioxidant 168 belongs to the phosphite antioxidant class, which mainly achieves the effect of antioxidant by decomposing hydroperoxides. Specifically, antioxidant 168 can react with hydroperoxides to convert free radicals into non-free radicals, relatively stable and inactive substances, thereby preventing hydroperoxides from further decomposing into free radicals and reducing the attack and damage of free radicals on the PVC molecular chain. This effect of decomposing hydroperoxides helps to delay the oxidative degradation process of PVC materials and maintain the stability of the physical properties and appearance of PVC materials. Antioxidant 1010 and antioxidant 168 are used together to further improve the antioxidant properties of PVC materials.
[0035] The acrylate processing aid is ACR401 or P551A.
[0036] Acrylate processing aids can promote the crushing and fusion of primary particles of PVC resin, increase the internal friction of PVC particles and the movement of molecular chains, accelerate the melting and plasticizing process of PVC resin, shorten the plasticizing time, increase the production rate, and improve the size and structural stability of PVC products.
[0037] The mineral filler is spherical nano active calcium with a particle size of D 50 In ≤1.0μm.
[0038] The preferred particle size D 50 Spherical nano calcium carbonate with a size of ≤1.0μm can improve the mechanical properties of PVC materials, and the nanostructure size effect and large specific surface area can enhance the interfacial bonding force with the PVC matrix, improve the toughness of PVC materials, and improve the fluidity of PVC materials.
[0039] The method for preparing the low-odor, environmentally friendly German standard 105°C low-voltage automotive wire PVC insulating material comprises firstly weighing the raw materials according to the formula, and then producing according to the following steps:
[0040] 1) First, fully mix the PVC resin, calcium zinc stabilizer, lubricant and antioxidant;
[0041] Then, add trioctyl trimellitate and continue mixing until the material temperature reaches 80°C;
[0042] Finally, porous ceramic and mineral fillers are added and mixed continuously until the material temperature reaches 120° C. to obtain a mixed material;
[0043] 2) Cooling and drying the mixture obtained in step 1), kneading and granulating, and then obtaining the desired PVC insulating material.
[0044] In step 1), PVC resin, calcium zinc stabilizer, lubricant and antioxidant are mixed in a high-speed mixer, the speed of the high-speed mixer is 300 rpm, and the mixing time is 120 seconds;
[0045] After adding trioctyl trimellitate, increase the speed of the high-speed mixer to 1250rpm. After the material temperature reaches 80℃, reduce the speed of the high-speed mixer to 200rpm, and then add porous ceramics and mineral fillers;
[0046] Then increase the speed of the high-speed mixer to 1250 rpm, until the material temperature reaches 130°C, then reduce the speed of the high-speed mixer to 200 rpm, open the discharge valve, and obtain the mixed material.
[0047] In step 2), the mixed material obtained in step 1) is fed into a twin-screw extruder of a two-stage granulation unit for mixing, and the obtained material is then extruded by a single screw of the two-stage granulation unit to form particles, thereby obtaining a PVC insulating material; wherein:
[0048] The speed of the twin-screw extruder is 260 rpm to 320 rpm; the temperature of the twin-screw extruder is controlled at 165°C to 175°C;
[0049] The temperatures of the two zones of the single-screw extruder are 110°C to 120°C and 120°C to 130°C respectively; the feeding speed of the single-screw extruder is 35 to 40 rpm.
[0050] Advantages of the invention:
[0051] The low-odor, environment-friendly German standard 105°C low-voltage automotive wire PVC insulating material of the present invention improves or even overcomes the problem of strong odor and high organic volatile content of PVC materials at high temperatures.
[0052] (1) The present invention defines the technical parameters of stabilizers and plasticizers, which are the main sources of odor in PVC materials except PVC resin. The total carbon release of the stabilizer at 120℃×4h is ≤100μg·C / g, which is lower than the total carbon release of calcium zinc stabilizer commonly used in PVC insulation materials within 4 hours (d≥1000μg·C / g). The total ester content of odor in plasticizer TOTM is ≥99.5%, the content of 2-ethylhexanol is ≤100mg / kg, the content of di(2-ethylhexyl) phthalate is ≤50mg / kg, and the content of dioctyl terephthalate is ≤0.6%.
[0053] (2) The porous ceramic structure of the deodorant, through nano-assembly and surface modification, has a large adsorption capacity and a fast adsorption rate for volatile organic substances. After the volatile organic compound molecules enter the internal space of the pores, they propagate in the specific mesoporous structure and microporous pores, and achieve physical adsorption and solidification through the force of the van der Waals electrostatic field, and desorption occurs below 150°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 This is a diagram of the microscopic structure of a deodorant.
[0055] Figure 2 It is a schematic diagram of the structure of the template. DETAILED DESCRIPTION
[0056] The present invention is described in detail below in conjunction with embodiments, but the specific embodiments of the present invention are not limited thereto and should cover the entire scope of the claims of the present invention.
[0057] In order to better compare the effects of raw material ratios on product performance, the raw materials used in each example have the same manufacturer, model / brand, etc.
[0058] The degree of polymerization of polyvinyl chloride resin is 1250-1350, and the number of "fish eyes" is ≤10 / 400cm 2 , purchased from Taizhou Liancheng Chemical Industry Co., Ltd., model US-70.
[0059] In order to control the odor in the formula, the following requirements are made for the odor-influencing indicators of TOTM:
[0060] ① Ester content ≥99.5%
[0061] ②2-Ethylhexanol content ≤ 100mg / kg
[0062] ③Di(2-ethylhexyl)phthalate content ≤50mg / kg
[0063] ④Dioctyl terephthalate ≤ 0.6%
[0064] Plasticizers meet the above four control points that affect the odor size at the same time. Manufacturers that meet this technical requirement include Jiangsu Zhengdan Chemical Industry Co., Ltd.'s trioctyl trimellitate (TOTM) product.
[0065] The deodorant is a porous ceramic structure. Through nano-assembly and surface modification, the porous ceramic has a large adsorption capacity and a fast adsorption rate for volatile organic substances. After the volatile organic molecules enter the internal space of the pores, they propagate in the specific mesoporous structure and microporous pores, and achieve physical adsorption and solidification through the force of the van der Waals electrostatic field, and there is no desorption below 150°C.
[0066] See attached for the microstructure of the deodorant Figure 1 , purchased from Shandong Guoci Functional Materials Co., Ltd., brand name TMA-100.
[0067] Environmentally friendly calcium zinc stabilizer, purchased from Changzhou Youjia New Material Technology Co., Ltd., brand K9026. The stabilizer product has a low odor level, and the total carbon release at 120℃×4h is ≤100μg·C / g.
[0068] Polyethylene wax, model LP0100P, purchased from SCG;
[0069] Calcium stearate was purchased from Anhui Ruihua New Materials Co., Ltd.;
[0070] Antioxidant 1010, a hindered phenol antioxidant, has a molecular weight of 1178 and was purchased from BASF;
[0071] Antioxidant 168, a phosphite antioxidant, with a molecular weight of 647, was purchased from BASF;
[0072] The nano mineral filler is spherical nano active calcium with a particle size of D 50 ≤1.0μm. Purchased from Jiangxi Guangyuan Chemical Co., Ltd., brand GY-916;
[0073] Processing aid P551A was purchased from Mitsubishi Chemical, Japan.
[0074] Preparation steps of each PVC insulation material:
[0075] 1) Put PVC resin, stabilizer and lubricant into a high-speed mixer, mix for 120 seconds at a speed of 300 rpm, add plasticizer, start the high speed at 1250 rpm, wait until the material temperature reaches 80°C, reduce the high-speed mixer speed by 200 rpm, add deodorant and nano mineral filler, start the high speed at 1250 rpm, reduce the speed by 200 rpm after the material temperature in the high-speed mixer reaches 130°C, open the discharge valve, and obtain a mixed material;
[0076] 2) The mixed material obtained in step 1) is discharged into a cold mixer using cooling water as a cooling medium. After the dry mixed material is cooled to 60° C., the cooled dry mixed material is discharged into a forced feeding bin of a twin-screw extruder.
[0077] 3) The material obtained in step 2) is extruded into particles by a single screw of a two-stage granulator unit to obtain low-odor, environmentally friendly 105°C low-voltage PVC insulating material for automotive wires; wherein the speed of the twin-screw extruder is 260 rpm to 320 rpm; the body of the twin-screw extruder is controlled at 165°C to 175°C; the temperatures of the two zones of the single-screw extruder body are 150°C to 160°C and 160°C to 170°C respectively; and the feeding speed of the single-screw extruder is 35 to 40 rpm.
[0078] Finally, the PVC insulation material obtained in step 3) is put into a ψ45+60 extruder and extruded onto the conductor to produce a conductor with a cross-sectional area of 0.35mm of the FLRY-B standard. 2 For the automotive line, samples are sent for testing of odor levels in accordance with BYD corporate standards (Q / BYDQ-A1901.404-2018).
[0079] The FLRY-B standard is a quality standard for wires and cables used in automotive wiring harness manufacturing. FLRY-B is one of the standards established by the German Automotive Industry Standards (VDA).
[0080] The first group of experiments discussed the effect of porous ceramic dosage on the performance of PVC insulation materials when the raw materials such as PVC resin and calcium zinc stabilizer are the same and the dosage of TOTM is slightly different:
[0081] Table 1 Specific examples
[0082] materials Number of copies Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Comparative Example 2 PVC resin 100 100 100 100 100 100 100 100 Calcium zinc stabilizer 5~12 8 8 8 8 8 8 8 TOTM 30~70 48 48 48 50 52 48 52 Porous ceramic deodorizer 2~6 2 3 4 4 6 0 0 Polyethylene wax 0.2~0.8 0.3 0.3 0.3 0.3 0.3 0.3 0.3 Calcium stearate 0.2~0.8 0.3 0.3 0.3 0.3 0.3 0.3 0.3 Antioxidant 1010 0.2~0.8 0.3 0.3 0.3 0.3 0.3 0.3 0.3 Antioxidant 168 0.2~0.8 0.3 0.3 0.3 0.3 0.3 0.3 0.3 Processing Aids 1~3 2 2 2 2 2 2 2 Mineral fillers 20~60 40 40 40 40 40 40 40
[0083] The test results are as follows:
[0084] Table 2 PVC insulation material performance test results
[0085]
[0086]
[0087] The odor level test is carried out in accordance with BYD's corporate standards. The test method is as follows:
[0088] (1) Take (20±2)g of the finished pellets and place them in a 1L odor bottle. Add 50mL of distilled water to the test container of test condition 1. Avoid contact between the sample in the test container and water. Store at room temperature (23±2)℃ for (24±1)h and then evaluate directly.
[0089] (2) No water is added to the test container. The test container should be tightly covered and placed in a preheated electric constant temperature air drying oven to heat to (40±2)℃ for (120±10)min before direct evaluation.
[0090] (3) No water is added to the test container. The test container should be tightly closed and placed in a preheated electric constant temperature air drying oven and heated to (65±2)℃ for (120±10)min. It should be cooled to room temperature for 2min. The odor bottle should be opened at 45° and the nose should be close to the opening to smell and make an evaluation within 10 seconds.
[0091] (4) No water is added to the test container. The test container should be tightly closed and placed in a preheated electric constant temperature air drying oven and heated to (80±2)℃ for (120±10)min. It should be cooled to room temperature for 5min. The odor bottle should be opened at 45° and the nose should be close to the opening to smell and make an evaluation within 10 seconds.
[0092] Table 3 PVC insulation material and FLRY-B 0.35mm 2 Smell test
[0093]
[0094] Case 1 to Case 3, when the same amount of plasticizer and deodorant was added, the automotive wire FLRY-B0.35mm 2 Odor: Under the test conditions of 23℃ and 40℃, the automotive wires were odorless, but under the test conditions above 65℃, they began to have an odor, but met the technical requirements of ≤3.5. In Case 4 and Case 5, the odor was significantly reduced as the amount of deodorant added increased.
[0095] The automotive wire FLRY-B 0.35mm made of Comparative Example 1 and Comparative Example 2 without adding deodorant 2 Under the test conditions of 23℃ and 40℃, the automotive wires have a noticeable odor, but the interference is not strong. The odor level is between 3.0-3.5. Under the test conditions of more than 65℃, the odor increases significantly, reaching level 4.5.
[0096] The second group of experiments: In the following experiments, using the same amount of PVC resin and porous ceramics as in Example 3, discuss the effects of the amount of other raw materials on the mechanical properties and insulating properties of PVC insulation materials.
[0097] Table 4 Specific examples
[0098] materials Number of copies Example 3 Example 6 Example 7 Example 8 PVC resin 100 100 100 100 100 Calcium zinc stabilizer 5~12 8 5 6 12 TOTM 30~70 48 70 30 40 Porous ceramic deodorizer 2~6 4 4 4 4 Polyethylene wax 0.2~0.8 0.3 0.8 0.4 0.2 Calcium stearate 0.2~0.8 0.3 0.6 0.8 0.2 Antioxidant 1010 0.2~0.8 0.3 0.2 0.6 0.8 Antioxidant 168 0.2~0.8 0.3 0.3 0.2 0.8 Processing Aids 1~3 2 2 1 3 Mineral fillers 20~60 40 60 20 30
[0099] The test results are as follows:
[0100] Table 5 PVC insulation material performance test results
[0101]
[0102]
[0103] In the second group of experiments, the ratio of PVC resin and porous ceramics was the same, the requirements for factors affecting odor such as plasticizer TOTM and calcium zinc stabilizer were high, and the results of odor tests all met the requirements. According to the mechanical properties and insulation properties tests in Table 5, both types of properties were qualified when the ratio of each additive changed.
Claims
1. A low-odor, environmentally friendly German standard 105°C low-voltage automotive wire PVC insulation material, characterized by: The following raw materials are included by weight: PVC resin: 100 parts, Calcium zinc stabilizer: 5-12 parts, Trioctyl trimellitate TOTM: 30-70 parts, Porous ceramic adsorbent: 2 to 6 parts, Lubricant: 0.4-1.6 parts, Antioxidant: 0.4-1.6 parts, Acrylate processing aid: 1 to 3 parts, Mineral filler: 20-60 parts; in: The polymerization degree of the PVC resin is 1250-1350, the number of impurity particles is ≤20, and the number of "fish eyes" is ≤15 / 400cm 2 , water extract conductivity ≤5S2cm1; The requirement for the calcium zinc stabilizer is that the total carbon release at 120°C×4h is ≤100μg·C / g; The requirements of the trioctyl trimellitate TOTM product include: ester content ≥ 99.5%, 2-ethylhexanol content ≤ 100 mg / kg, di(2-ethylhexyl) phthalate content ≤ 50 mg / kg and dioctyl terephthalate ≤ 0.6%; The microstructure of the porous ceramic adsorbent is a regular pipeline structure, the pipeline diameter is nanometer-level, the pipeline is a spatial network structure, and a surfactant with affinity to VOC is attached in the pipeline.
2. The low-odor, environmentally friendly German standard 105°C low-voltage automotive wire PVC insulation material according to claim 1 is characterized in that The lubricant comprises: polyethylene wax: 0.2-0.8 parts and calcium stearate: 0.2-0.8 parts.
3. The low-odor, environmentally friendly German standard 105°C low-voltage automotive wire PVC insulation material according to claim 1 is characterized in that The antioxidants include hindered phenol antioxidants and phosphite antioxidants.
4. The low-odor, environmentally friendly German standard 105°C low-voltage automotive wire PVC insulation material according to claim 1 is characterized in that The acrylate processing aid is ACR 401 or P551A.
5. The low-odor, environmentally friendly German standard 105°C low-voltage automotive wire PVC insulation material according to claim 1 is characterized in that The mineral filler is spherical nano active calcium with a particle size of D 50 In ≤1.0μm.
6. The method for preparing the PVC insulating material according to any one of claims 1 to 5, characterized in that: First, weigh the raw materials according to the formula, and then produce according to the following steps: 1) First, fully mix the PVC resin, calcium zinc stabilizer, lubricant and antioxidant; Then, add trioctyl trimellitate and continue mixing until the material temperature reaches 80°C; Finally, porous ceramic and mineral fillers are added and mixed continuously until the material temperature reaches 120° C. to obtain a mixed material; 2) Cooling and drying the mixture obtained in step 1), kneading and granulating, and then obtaining the desired PVC insulating material.
7. The method for preparing PVC insulating material according to claim 6, characterized in that In step 1), PVC resin, calcium zinc stabilizer, lubricant and antioxidant are mixed in a high-speed mixer, the speed of the high-speed mixer is 300 rpm, and the mixing time is 120 seconds; After adding trioctyl trimellitate, increase the speed of the high-speed mixer to 1250rpm. After the material temperature reaches 80℃, reduce the speed of the high-speed mixer to 200rpm, and then add porous ceramics and mineral fillers; Then increase the speed of the high-speed mixer to 1250 rpm, until the material temperature reaches 130°C, then reduce the speed of the high-speed mixer to 200 rpm, open the discharge valve, and obtain the mixed material.
8. The method for preparing PVC insulating material according to claim 6, characterized in that In step 2), the mixed material obtained in step 1) is fed into a twin-screw extruder of a two-stage granulation unit for mixing, and the obtained material is then extruded by a single screw of the two-stage granulation unit to form particles, thereby obtaining a PVC insulating material; wherein: The speed of the twin-screw extruder is 260 rpm to 320 rpm; the temperature of the twin-screw extruder is controlled at 165°C to 175°C; The temperatures of the two zones of the single-screw extruder are 110°C to 120°C and 120°C to 130°C respectively; the feeding speed of the single-screw extruder is 35 to 40 rpm.