Preparation method for high-molecular polymer all-plastic simulation wood material based on essential oil microcapsules

By combining essential oil microcapsules with polymer composite plastic elastomers in all-plastic simulated wood materials, the problem of lack of wood odor in all-plastic simulated wood is solved, and the environmentally friendly characteristics of slow release of odor and recycling are achieved.

CN118879094APending Publication Date: 2024-11-01GUANGDONG JUWEI NEW MATERIALS R&D CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411283269.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing fully plastic simulated wood products lack wood odor, cannot adhere to essential oils, and the odor is short-lived, and cannot replace the odor characteristics of real wood.

Method used

In the preparation process of polymer fully plastic simulated wood materials, essential oil microcapsules are combined with polymer composite plastic elastomer, and the essential oil microcapsules are evenly distributed in the process of hot pressing, kneading, pressing and embossing. In the material, the aroma is slowly released.

Benefits of technology

It has achieved the effect of fully plastic simulated wood material with wood odor, supports recycling and environmentally friendly carbon reduction, and can adopt traditional wood processing methods to enhance the economic and social value of the products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879094A_ABST
    Figure CN118879094A_ABST
Patent Text Reader

Abstract

The invention belongs to wood-like building materials, and particularly relates to a method for preparing a high-molecular polymer all-plastic simulation wood material based on essential oil microcapsules, which comprises the steps of preparing a high-molecular polymer composite plastic elastomer, preparing an all-plastic simulation wood material and preparing the essential oil microcapsules for the all-plastic simulation wood material. The all-plastic simulation wood material is simple in structure and ingenious in design, adopts a high-molecular polymer plastic connection polymerization mode, is good in smell effect, can be recycled all the time through a traditional wood processing method, and is high in practicability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to wood-like building materials, and in particular relates to a preparation method of a macromolecular polymer all-plastic simulated wood material based on essential oil microcapsules. Background Art

[0003] Existing all-plastic simulated wood products have become odorous wood to replace real wood, because all-plastic simulated wood only has the appearance of wood, but does not have the smell of wood. Since all-plastic simulated wood is based on plastic, any essential oil cannot adhere to the all-plastic simulated wood material. Even if it adheres to the all-plastic simulated wood, the smell will disappear quickly. Summary of the invention

[0004] The purpose of the present invention is to add essential oil microcapsules during the production process of plastic wood or all-plastic simulated wood materials, so that the plastic wood or all-plastic simulated wood materials have the smell of wood. The essential oil microcapsules are used in the preparation steps of the all-plastic simulated wood materials, the preparation process is reasonable, the design is ingenious, and the polymer connection polymerization method is adopted to make the all-plastic simulated wood materials have a good smell effect. The traditional wood processing method can also be used, and it can be recycled and reused all the time, which is highly practical.

[0005] In order to solve the above problems, the present invention relates to a method for preparing a polymer all-plastic simulated wood material based on essential oil microcapsules, comprising the following steps: (1) Preparation of polymer composite plastic elastomers Weigh the raw materials according to the following weight proportions: 50-60 parts of polystyrene, 30-40 parts of high-density polyethylene, and 15-25 parts of polyethylene terephthalate; mix the weighed raw materials and put them into a hot autoclave for hot pressing at a temperature of 180-200° C. and a time of 5-7 min; the hot-pressed materials enter a tower reactor at a reaction temperature of 150-160° C. and a time of 5-10 min; the reacted materials enter a kneading machine for kneading at a kneading temperature of 90-120° C. and a time of 3-5 min; after kneading, a polymer composite plastic elastic body is obtained, and the melting point of the polymer composite plastic elastomer is 150° C.; (2) Preparation of all-plastic simulated wood materials Weigh the following raw materials in parts by weight: 80 parts of high molecular polymer recycled material and 20 parts of high molecular polymer composite plastic elastomer, put the weighed high molecular polymer recycled material and high molecular polymer composite plastic elastomer into a kneading machine for kneading at a temperature of 200° C. for 10-15 minutes to obtain material A; Material A is put into a special-shaped extruder for processing to obtain material B; A single screw or twin screw is used to extrude material B onto a temperature-controlled mold. The mold temperature is 200°C and the molding time is 30 seconds. After molding, the material is cooled and shaped to obtain a finished product D. A circulating water cooling system is used for cooling and shaping. The cooling temperature is 60-90°C. Finished product D is micro-sprayed with essential oil microcapsule material at a temperature of 60°C to form finished product E, and finished product E is put into a thermal transfer embossing device for embossing treatment at a temperature of 60°C. After embossing, it is cut to a fixed length to become a full-plastic simulated wood product, and is packaged and shipped after passing the inspection; Unqualified products and scraps from the preparation process are put into the crusher for processing.

[0006] Preferably, during the preparation of the high molecular polymer composite plastic elastomer, the raw materials are weighed according to the following weight proportions: 55 parts of polystyrene, 35 parts of high density polyethylene, and 20 parts of polyethylene terephthalate.

[0007] Preferably, the essential oil microcapsule material is made of polystyrene and is made of semi-closed essential oil microcapsules, and the essential oil slowly releases its aroma through a semipermeable membrane.

[0008] Compared with the prior art, the technical solution of the present invention has the following advantages: 1. Make the all-plastic simulated wood material have an odor, replace real wood, and can be recycled and reused after use. It has extremely high economic and social value, and has the characteristics of environmental protection, carbon reduction and circular economy.

[0009] 2. Related high molecular polymers and recycled wood can be processed to generate odor.

[0010] 3. Essential oil microcapsule all-plastic simulated wood materials can be used using traditional woodworking methods, without the need to add special methods and accessories such as clamps or support frames. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is a process flow chart of an embodiment.

[0012] Figure 2 It is a schematic cross-sectional view of product E.

[0013] Figure 3 Schematic diagram of essential oil microcapsules. DETAILED DESCRIPTION

[0014] In order to make the technical purpose, technical solution and beneficial effects of the present invention clearer, the technical solution of the present invention is further described below in conjunction with specific embodiments.

[0015] Example 1: A method for preparing a polymer all-plastic simulated wood material based on essential oil microcapsules, such as Figure 1-3As shown, the following steps are included: (1) Preparation of polymer composite plastic elastomers Weigh the raw materials according to the following weight proportions: 50 parts of polystyrene, 30 parts of high-density polyethylene, and 15 parts of polyethylene terephthalate; mix the weighed raw materials and put them into a hot autoclave for hot pressing at a temperature of 180° C. and a time of 5 minutes; the hot-pressed materials enter a tower reactor at a reaction temperature of 150° C. and a time of 5-10 minutes; the reacted materials enter a kneading machine for kneading at a kneading temperature of 90° C. and a time of 3 minutes; after kneading, a high-molecular polymer composite plastic elastomer is obtained, and the melting point of the high-molecular polymer composite plastic elastomer is 150° C.; (2) Preparation of all-plastic simulated wood materials Weigh the following raw materials in parts by weight: 80 parts of high molecular polymer recycled material and 20 parts of high molecular polymer composite plastic elastomer, put the weighed high molecular polymer recycled material and high molecular polymer composite plastic elastomer into a kneading machine for kneading at a temperature of 200° C. for 10 minutes to obtain material A; Material A is put into a special-shaped extruder for processing to obtain material B; A single screw or twin screw is used to extrude material B onto a temperature-controlled mold. The mold temperature is 200°C and the molding time is 30 seconds. After molding, the material is cooled and shaped to obtain a finished product D. The cooling and shaping process uses a circulating water cooling system at a cooling temperature of 60°C. Finished product D is micro-sprayed with essential oil microcapsule material at a temperature of 60°C. The essential oil microcapsule material is made of polystyrene and is made of semi-enclosed essential oil microcapsules. The essential oil slowly releases the aroma through a semi-permeable membrane. Conventional preparation methods of microcapsules include: complex coacervation, single coacervation, interfacial polymerization, in-situ polymerization, etc. Finished product E is formed, and finished product E is put into a thermal transfer embossing device for embossing treatment. The embossing temperature is 60°C. After embossing, it is cut to a fixed length to become a fully plastic simulated wood product, which is packaged and shipped after passing the inspection; Unqualified products and scraps from the preparation process are put into the crusher for processing.

[0016] Embodiment 2: A method for preparing a polymer all-plastic simulated wood material based on essential oil microcapsules, comprising the following steps: (1) Preparation of polymer composite plastic elastomers Weigh the raw materials according to the following weight proportions: 60 parts of polystyrene, 40 parts of high-density polyethylene, and 25 parts of polyethylene terephthalate; mix the weighed raw materials and put them into a hot autoclave for hot pressing at a temperature of 200° C. and a time of 7 minutes; the hot-pressed materials enter a tower reactor at a reaction temperature of 160° C. and a time of 10 minutes; the reacted materials enter a kneading machine for kneading at a kneading temperature of 120° C. and a time of 5 minutes; after kneading, a high-molecular polymer composite plastic elastomer is obtained, and the melting point of the high-molecular polymer composite plastic elastomer is 150° C.; (2) Preparation of all-plastic simulated wood materials Weigh the following raw materials in parts by weight: 80 parts of high molecular polymer recycled material and 20 parts of high molecular polymer composite plastic elastomer, put the weighed high molecular polymer recycled material and high molecular polymer composite plastic elastomer into a kneading machine for kneading at a temperature of 200° C. for 15 minutes to obtain material A; Material A is put into a special-shaped extruder for processing to obtain material B; A single screw or twin screw is used to extrude material B onto a temperature-controlled mold. The mold temperature is 200°C and the molding time is 30 seconds. After molding, the material is cooled and shaped to obtain a finished product D. The cooling and shaping process uses a circulating water cooling system at a cooling temperature of 90°C. Finished product D is micro-sprayed with essential oil microcapsule material at a temperature of 60° C. The essential oil microcapsule material is made of polystyrene and is made of semi-enclosed essential oil microcapsules. The essential oil slowly releases fragrance through a semipermeable membrane. Conventional preparation methods of microcapsules include: complex coacervation, single coacervation, interfacial polymerization, in-situ polymerization, etc. to form finished product E. Finished product E is put into a thermal transfer embossing device for embossing treatment at a temperature of 60° C. After embossing, it is cut to a fixed length to become a fully plastic simulated wood product, which is packaged and shipped after passing inspection; Unqualified products and scraps from the preparation process are put into the crusher for processing.

[0017] Embodiment 3: A method for preparing a polymer all-plastic simulated wood material based on essential oil microcapsules, comprising the following steps: (1) Preparation of polymer composite plastic elastomers Weigh the raw materials according to the following weight proportions: 50 parts of polystyrene, 40 parts of high-density polyethylene, and 15 parts of polyethylene terephthalate; mix the weighed raw materials and put them into a hot autoclave for hot pressing at a temperature of 200° C. and a time of 5 minutes; the hot-pressed materials enter a tower reactor at a reaction temperature of 160° C. and a time of 5 minutes; the reacted materials enter a kneading machine for kneading at a kneading temperature of 120° C. and a time of 3 minutes; after kneading, a high-molecular polymer composite plastic elastomer is obtained, and the melting point of the high-molecular polymer composite plastic elastomer is 150° C.; (2) Preparation of all-plastic simulated wood materials Weigh the following raw materials in parts by weight: 80 parts of high molecular polymer recycled material and 20 parts of high molecular polymer composite plastic elastomer, put the weighed high molecular polymer recycled material and high molecular polymer composite plastic elastomer into a kneading machine for kneading at a temperature of 200° C. for 15 minutes to obtain material A; Material A is put into a special-shaped extruder for processing to obtain material B; A single screw or twin screw is used to extrude material B onto a temperature-controlled mold. The mold temperature is 200°C and the molding time is 30 seconds. After molding, the material is cooled and shaped to obtain a finished product D. The cooling and shaping process uses a circulating water cooling system at a cooling temperature of 60°C. Finished product D is micro-sprayed with essential oil microcapsule material at a temperature of 60° C. The essential oil microcapsule material is made of polystyrene and is made of semi-enclosed essential oil microcapsules. The essential oil slowly releases fragrance through a semipermeable membrane. Conventional preparation methods of microcapsules include: complex coacervation, single coacervation, interfacial polymerization, in-situ polymerization, etc. to form finished product E. Finished product E is put into a thermal transfer embossing device for embossing treatment at a temperature of 60° C. After embossing, it is cut to a fixed length to become a fully plastic simulated wood product, which is packaged and shipped after passing inspection; Unqualified products and scraps from the preparation process are put into the crusher for processing.

[0018] Embodiment 4: A method for preparing a polymer all-plastic simulated wood material based on essential oil microcapsules, comprising the following steps: (1) Preparation of polymer composite plastic elastomers Weigh the raw materials according to the following weight proportions: 55 parts of polystyrene, 35 parts of high-density polyethylene, and 20 parts of polyethylene terephthalate; mix the weighed raw materials and put them into a hot autoclave for hot pressing at a temperature of 190° C. and a time of 6 minutes; the hot-pressed materials enter a tower reactor at a reaction temperature of 155° C. and a time of 8 minutes; the reacted materials enter a kneading machine for kneading at a kneading temperature of 100° C. and a time of 4 minutes; after kneading, a high-molecular polymer composite plastic elastomer is obtained, and the melting point of the high-molecular polymer composite plastic elastomer is 150° C.; (2) Preparation of all-plastic simulated wood materials Weigh the following raw materials in parts by weight: 80 parts of high molecular polymer recycled material and 20 parts of high molecular polymer composite plastic elastomer, put the weighed high molecular polymer recycled material and high molecular polymer composite plastic elastomer into a kneading machine for kneading at a temperature of 200° C. for 12 minutes to obtain material A; Material A is put into a special-shaped extruder for processing to obtain material B; A single screw or twin screw is used to extrude material B onto a temperature-controlled mold. The mold temperature is 200°C and the molding time is 30 seconds. After molding, the material is cooled and shaped to obtain a finished product D. The cooling and shaping process uses a circulating water cooling system with a cooling temperature of 75°C. Finished product D is micro-sprayed with essential oil microcapsule material at a temperature of 60° C. The essential oil microcapsule material is made of polystyrene and is made of semi-enclosed essential oil microcapsules. The essential oil slowly releases fragrance through a semipermeable membrane. Conventional preparation methods of microcapsules include: complex coacervation, single coacervation, interfacial polymerization, in-situ polymerization, etc. to form finished product E. Finished product E is put into a thermal transfer embossing device for embossing treatment at a temperature of 60° C. After embossing, it is cut to a fixed length to become a fully plastic simulated wood product, which is packaged and shipped after passing inspection; Unqualified products and scraps from the preparation process are put into the crusher for processing.

[0019] Among the above embodiments, Embodiment 4 is the best embodiment.

[0020] Finally, it should be noted that the above embodiments are only used to illustrate but not limit the technical solutions of the present invention, and any equivalent substitutions of the present invention and any modifications or partial substitutions that do not depart from the spirit and scope of the present invention should be included in the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a polymer all-plastic simulated wood material based on essential oil microcapsules, characterized in that: The following steps are involved: (1) Preparation of polymer composite plastic elastomers Weigh the raw materials according to the following weight proportions: 50-60 parts of polystyrene, 30-40 parts of high-density polyethylene, and 15-25 parts of polyethylene terephthalate; mix the weighed raw materials and put them into a hot autoclave for hot pressing at a temperature of 180-200° C. and a time of 5-7 min; the hot-pressed materials enter a tower reactor at a reaction temperature of 150-160° C. and a time of 5-10 min; the reacted materials enter a kneading machine for kneading at a kneading temperature of 90-120° C. and a time of 3-5 min; after kneading, a polymer composite plastic elastic body is obtained, and the melting point of the polymer composite plastic elastomer is 150° C.; (2) Preparation of all-plastic simulated wood materials Weigh the following raw materials in parts by weight: 80 parts of high molecular polymer recycled material and 20 parts of high molecular polymer composite plastic elastomer, put the weighed high molecular polymer recycled material and high molecular polymer composite plastic elastomer into a kneading machine for kneading at a temperature of 200° C. for 10-15 minutes to obtain material A; Material A is put into a special-shaped extruder for processing to obtain material B; A single screw or twin screw is used to extrude material B onto a temperature-controlled mold. The mold temperature is 200°C and the molding time is 30 seconds. After molding, the material is cooled and shaped to obtain a finished product D. A circulating water cooling system is used for cooling and shaping. The cooling temperature is 60-90°C. Finished product D is micro-sprayed with essential oil microcapsule material at a temperature of 60°C to form finished product E, and finished product E is put into a thermal transfer embossing device for embossing treatment at a temperature of 60°C. After embossing, it is cut to a fixed length to become a full-plastic simulated wood product, and is packaged and shipped after passing the inspection; Unqualified products and scraps from the preparation process are put into the crusher for processing.

2. The method for preparing a polymer all-plastic simulated wood material based on essential oil microcapsules according to claim 1, characterized in that: During the preparation of the high molecular polymer composite plastic elastomer, the raw materials are weighed according to the following weight parts: 55 parts of polystyrene, 35 parts of high density polyethylene, and 20 parts of polyethylene terephthalate.

3. The method for preparing a polymer all-plastic simulated wood material based on essential oil microcapsules according to claim 1, characterized in that: The essential oil microcapsule material is made of polystyrene and is made of semi-closed essential oil microcapsules. The essential oil slowly releases its fragrance through a semi-permeable membrane.