Long-acting anticorrosive water-based paint and preparation method thereof

By using combined materials such as aqueous acrylic resin, aqueous EVA emulsion and modified glass flakes in water-based coatings, the problem of poor corrosion resistance in low-temperature environments is solved, and the improvement of high temperature resistance and corrosion resistance is achieved, which extends the The service life of the coating.

CN118879140AInactive Publication Date: 2024-11-01ZHENJIANG YONGYI NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411105075.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional water-based anticorrosion coatings are prone to water absorption, increased viscosity, decreased leveling and coating rupture in low-temperature environments, which affect their anticorrosion performance and service life.

Method used

Using a combination of aqueous acrylic resin, aqueous EVA emulsion, modified glass flakes, leveling agent, defoaming agent, thickening agent and anti-rust pigment, the anti-corrosion performance and resistance of the coating are improved through the preparation and stirring process of modified glass flakes. Low temperature performance.

Benefits of technology

It significantly improves the corrosion resistance and low temperature resistance of the coating, enhances the adhesion and permeability of the coating, extends the service life, and maintains good smoothness and corrosion resistance under low temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879140A_ABST
    Figure CN118879140A_ABST
Patent Text Reader

Abstract

The invention provides a long-acting anticorrosive water-based paint and a preparation method thereof, and belongs to the technical field of paints. Comprising the following raw material components: 40-50 parts of water-based acrylic resin, 7-11 parts of a water-based EVA emulsion, 8-13 parts of modified glass flakes, 0.1-1 part of a leveling agent, 0.1-1 part of a defoaming agent, 20-35 parts of water, 0.1-0.5 part of a thickening agent and 5-10 parts of an anti-rust pigment. According to the invention, the water-based paint prepared by taking the water-based acrylic resin as the base material has excellent corrosion resistance and low temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a long-lasting anticorrosive water-based coating and a preparation method thereof. Background Art

[0002] Anticorrosive coatings play a decorative role and can protect the substrate from moisture, radiation, biological, mechanical and chemical corrosion in the air. The anticorrosion effect is affected by many factors, such as the performance of the paint film, the quality of the substrate, the interaction between the paint film and the substrate, and the degree of environmental corrosion. Traditional organic polymer coatings mainly include polyurethane, acrylic resin, epoxy resin, alkyd resin, etc. Water-based anticorrosive coatings mainly use water as a solvent and dispersant, and have the advantages of super weather resistance, heat resistance, solvent resistance, high hardness, weldability, non-flammable, non-explosive, and zero VOC emissions.

[0003] However, water-based paints have inherent performance defects. For example, water-based paints contain water-based acrylic resins, which are hydrophilic and will absorb water during long-term use. They are easily damaged or lose their anti-corrosion function due to the influence of the external environment. In addition, water-based acrylic resins have poor low-temperature resistance. Under low-temperature conditions, the viscosity increases and the leveling property decreases, affecting the smoothness and aesthetics of the coating. When used at low temperatures, the coating on the surface of the specimen will crack, affecting the service life of the specimen.

[0004] Therefore, it is an issue worthy of study to provide a long-lasting anticorrosive water-based coating having good anticorrosion performance and good low-temperature resistance when used in a low-temperature environment and a preparation method thereof. Summary of the invention

[0005] In order to solve the problems existing in the background technology, the present invention provides a long-lasting anti-corrosion water-based coating and a preparation method thereof, which ensures that the water-based coating prepared with water-based acrylic resin as the base material has both excellent anti-corrosion performance and low-temperature resistance.

[0006] In order to achieve the above-mentioned purpose, in a first aspect, the present invention provides a long-lasting anti-corrosion water-based coating, which comprises the following raw material components by weight: 40-50 parts of water-based acrylic resin, 7-11 parts of water-based EVA emulsion, 8-13 parts of modified glass flakes, 0.1-1 parts of leveling agent, 0.1-1 parts of defoaming agent, 20-35 parts of water, 0.1-0.5 parts of thickener and 5-10 parts of anti-rust pigment.

[0007] Furthermore, the preparation method of the modified glass flakes is as follows:

[0008] A1. Treat the surface of the glass flakes with an anionic surfactant, then rinse with deionized water and dry to obtain pretreated glass flakes;

[0009] A2. Add 30 g of mixed powder of NaF, KF and NH4F to 100 ml of 40% HF aqueous solution, and stir until completely dissolved to obtain an acid etching solution;

[0010] A3, put the pretreated glass flakes obtained in A1 into the acid etching solution obtained in A2, move the container into a super thermostat, immerse in a water bath at 25°C for 10-20s, take out, rinse with hot water, and dry to obtain acid-etched glass flakes;

[0011] A4. Prepare the surface treatment agent into a 1% aqueous solution by mass, and add the acid-etched glass flakes obtained in A3 into it, soaking them completely for 5 minutes, take them out and dry them, and the modified glass flakes are obtained.

[0012] Furthermore, in A1, the anionic surfactant is sodium dodecylbenzene sulfonate.

[0013] Furthermore, in A2, the mass ratio of NaF, KF and NH4F is (7-9):(3-5):1.

[0014] Furthermore, in A4, the surface treatment agent is silane coupling agent KH-550.

[0015] Furthermore, the leveling agent is an aromatic alkylsiloxane leveling agent.

[0016] Furthermore, the defoaming agent is a silicone defoaming agent.

[0017] Furthermore, the thickener is carboxymethyl cellulose.

[0018] Furthermore, the anti-rust pigment is any one of mica iron oxide, zinc phosphate, and aluminum tripolyphosphate.

[0019] In a second aspect, the present invention provides a method for preparing the above-mentioned long-lasting anticorrosive water-based coating, comprising the following steps:

[0020] S1, putting water-based acrylic resin and water-based EVA emulsion into a dispersion tank, controlling the temperature of the dispersion tank to 15-18° C., turning on the agitator, stirring at a speed of 220-260 r / min, and stirring for 18-30 min to uniformly mix the water-based acrylic resin and the water-based EVA emulsion to obtain a mixture a;

[0021] S2. Add modified glass flakes to the mixture a obtained in S1 under stirring, control the temperature of the dispersion tank to 20-24°C, adjust the stirring speed to 350-450r / min, stir for 12-18min, then adjust the stirring speed to 460-560r / min, stir for 16-24min, and obtain a mixture b;

[0022] S3. Under stirring, add leveling agent, defoaming agent, water, thickener and anti-rust pigment to the mixture b obtained in S2, control the temperature of the dispersion tank to 26-36°C, adjust the stirring speed to 280-340r / min, stir for 30-40min, cool, and obtain a long-lasting anticorrosive water-based coating.

[0023] This application has the following beneficial effects:

[0024] 1. The water-based EVA emulsion used in the present invention has good flexibility and low glass transition temperature. Its soft segment forms a flexible network in the coating film, providing necessary elasticity at low temperatures, thereby reducing the shrinkage and cracking of the coating caused by temperature drop, and improving the performance of the water-based acrylic resin in a low-temperature environment; at the same time, the water-based EVA emulsion and the water-based acrylic resin can also produce a certain synergistic effect, thereby improving the water resistance and anti-corrosion performance of the coating.

[0025] Glass flakes have the effect of enhancing mechanical strength and corrosion resistance. The acid-etched glass flakes have increased surface roughness and can better combine with water-based acrylic resin and water-based EVA emulsion, thereby improving the adhesion and permeability resistance of the coating, thereby improving the anti-corrosion performance; at the same time, protrusions are formed on the surface of the acid-etched glass flakes, making the penetration path of the corrosive medium in the coating tortuous and long, increasing the penetration time and energy required for the corrosive medium to reach the substrate, further improving the anti-corrosion performance.

[0026] 2. In the preparation of modified glass flakes, the acid-etched glass flakes are treated with surface treatment agent KH-550 to further improve the bonding strength between the glass flakes and the water-based acrylic resin and the water-based EVA emulsion, so that the cured film layer forms a solid overall film. The surface treatment agent used is like forming a molecular bridge between the water-based acrylic resin and the glass flakes, firmly connecting the two different materials together, thereby enhancing the anti-permeability (anti-corrosion) property.

[0027] The mechanical anchoring of glass flakes with water-based acrylic resin after acid etching is a physical bond, and the glass flakes treated with surface treatment agents are firmly bonded to the water-based acrylic resin through chemical bonding. The two work together, through the combination of physical bonding and chemical bonding, to make the glass flakes and water-based acrylic resin more firmly bonded, and synergistically improve the anti-corrosion performance.

[0028] 3. Experimental verification shows that the addition of water-based EVA emulsion can improve the low-temperature resistance of the water-based coating; adding glass flakes to the water-based EVA emulsion can improve the low-temperature resistance of the water-based coating; adding modified glass flakes to the water-based EVA emulsion can further improve the low-temperature resistance of the water-based coating.

[0029] If water-based EVA emulsion is not added, the addition of modified glass flakes will cause the low-temperature resistance of the water-based coating to decrease instead of increase. The inventors believe that the addition of glass flakes increases the hardness of the coating while reducing the toughness of the coating. Especially in low-temperature environments, coatings without EVA soft segments are more prone to local cracks, resulting in a more severe decline in coating performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 , a comparative trend chart of the test data of the anticorrosion performance (salt spray resistance) of the water-based coatings obtained in Examples 1-5 of the present invention and Comparative Examples 1-4;

[0031] Figure 2 , a trend chart comparing test data of low temperature resistance (low temperature loss rate of salt spray resistance) of water-based coatings obtained from Examples 1-5 of the present invention and Comparative Examples 1-4. DETAILED DESCRIPTION

[0032] The present application is further described in detail below with reference to the embodiments.

[0033] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.

[0034] Example 1: (1) First, prepare modified glass flakes, the steps are as follows:

[0035] A1. Treat the surface of the glass flakes with anionic surfactants. Specifically, completely immerse the glass flakes in the anionic surfactant for 1 hour, stirring intermittently during the process, in order to clean and activate the surface of the glass flakes, remove impurities and oil stains on the surface, and provide better reaction conditions for the subsequent acid etching step. Then, rinse the glass flakes treated with anionic surfactants with deionized water to remove excess anionic surfactants physically adsorbed, and ensure that all residual anionic surfactants are removed. The number of rinses depends on the actual situation. In this embodiment, rinse four times. Then, put the rinsed and drained glass flakes into an oven and dry them at 45°C for 35 minutes to obtain a clean and activated glass flake surface, which is the pretreated glass flake.

[0036] Among them, the anionic surfactant is sodium dodecylbenzene sulfonate (Kaixing K12), which was purchased from Guangdong Zhongrun Chemical Co., Ltd. Glass flakes (industrial grade, density 2.4g / cm 3 , purity 99%) was purchased from Lingshou County Yehui Mineral Products Co., Ltd.

[0037] A2. Add 30g of mixed powder of NaF, KF and NH4F to 100ml of 40% HF aqueous solution, and stir until completely dissolved (shake the container gently under sufficient light and observe the solution. If the solution looks clear and there are no visible solid particles, it can be judged as completely dissolved) to obtain an acid etching solution. The mass ratio of NaF, KF and NH4F is 8:4:1.

[0038] A3. Place the pretreated glass flakes obtained in A1 into the acid etching solution obtained in A2, move the container into a super thermostat, immerse in a water bath at 25°C for 15 seconds, take out, rinse with hot water until the rinse water is neutral, and then dry naturally at room temperature to obtain acid-etched glass flakes.

[0039] A4. Prepare the surface treatment agent into an aqueous solution with a mass fraction of 1%, and add the acid-etched glass flakes obtained in A3 into it, soak them completely for 5 minutes, take them out, and dry them in an oven at 45°C for 40 minutes to obtain modified glass flakes.

[0040] Among them, the surface treatment agent is silane coupling agent KH-550, which was purchased from Zhengzhou Lishengyuan Chemical Products Co., Ltd.

[0041] (2) Then, a long-lasting anticorrosive water-based coating is prepared, and the steps are as follows:

[0042] S1. Put 45 parts of water-based acrylic resin and 8 parts of water-based EVA emulsion into a dispersion tank by weight, control the temperature of the dispersion tank to 16° C., turn on the agitator, stir at a speed of 240 r / min, and stir for 22 min to uniformly mix the water-based acrylic resin and the water-based EVA emulsion to obtain a mixture a.

[0043] Among them, water-based acrylic resin (AA-8650S) was purchased from Suzhou Qingtian Chemical Co., Ltd. Water-based EVA emulsion (WK-638) was purchased from Dongguan Weike Chemical Co., Ltd.

[0044] S2. According to the same standard of parts by weight, add 10 parts of modified glass flakes to the mixture a obtained in S1 under stirring, control the temperature of the dispersion tank to 22°C, adjust the stirring speed to 390r / min, stirring time for 15min, then adjust the stirring speed to 490r / min, stirring time for 20min, to obtain a mixture b.

[0045] S3. According to the same standard weight parts, add 0.7 parts of leveling agent, 0.5 parts of defoaming agent, 28 parts of water, 0.3 parts of thickener and 7 parts of anti-rust pigment to the mixture b obtained in S2 under stirring, control the temperature of the dispersion tank to 30°C, adjust the stirring speed to 300r / min, stir for 35min, cool, and obtain a long-lasting anticorrosive water-based coating.

[0046] Among them, the leveling agent is BYK leveling agent (BYK307), the chemical composition is aryl alkyl modified polymethane siloxane, purchased from Dongguan Hengfeng New Materials Co., Ltd. The defoamer is an organic silicon defoamer (industrial grade, 10% content), purchased from Shandong Kasong New Materials Co., Ltd. The thickener is carboxymethyl cellulose (superior grade), purchased from Qingzhou Qingquan Cellulose Factory. The anti-rust pigment is mica iron oxide (industrial grade, 325 mesh), purchased from Lingshou County Jinbo Mineral Products Processing Plant.

[0047] Example 2: The difference between this example and Example 1 is that: (1) First, the modified glass flakes are prepared in the following steps:

[0048] A1. Treat the surface of the glass flakes with anionic surfactant, then wash and dry to obtain pretreated glass flakes.

[0049] A2. Add 30g of mixed powder of NaF, KF and NH4F to 100ml of 40% HF aqueous solution, stir until completely dissolved, and obtain an acid etching solution, wherein the mass ratio of NaF, KF and NH4F is 7:3:1.

[0050] A3. Place the pretreated glass flakes obtained in A1 into the acid etching solution obtained in A2, move the container into a super thermostat, immerse in a water bath at 25°C for 10 seconds, take out, rinse with hot water, and dry to obtain acid-etched glass flakes.

[0051] A4. Prepare the surface treatment agent into a 1% aqueous solution by mass, and add the acid-etched glass flakes obtained in A3 into it, soaking them completely for 5 minutes, take them out and dry them, and the modified glass flakes are obtained.

[0052] (2) Then, a long-lasting anticorrosive water-based coating is prepared, and the steps are as follows:

[0053] S1. Put 40 parts of water-based acrylic resin and 7 parts of water-based EVA emulsion into a dispersion tank by weight, control the temperature of the dispersion tank to 15° C., turn on the agitator, stir at a speed of 220 r / min, and stir for 18 min to uniformly mix the water-based acrylic resin and the water-based EVA emulsion to obtain a mixture a.

[0054] S2. According to the same standard of parts by weight, add 13 parts of modified glass flakes to the mixture a obtained in S1 under stirring, control the temperature of the dispersion tank to 24°C, adjust the stirring speed to 450r / min, and stir for 18min, then adjust the stirring speed to 560r / min, and stir for 24min to obtain a mixture b.

[0055] S3. According to the same standard weight parts, add 0.1 parts of leveling agent, 0.1 parts of defoaming agent, 20 parts of water, 0.1 parts of thickener and 5 parts of anti-rust pigment to the mixture b obtained in S2 under stirring, control the temperature of the dispersion tank to 26°C, adjust the stirring speed to 280r / min, stir for 30min, cool, and obtain a long-lasting anticorrosive water-based coating.

[0056] Example 3: The difference between this example and Example 1 is that: (1) First, the modified glass flakes are prepared in the following steps:

[0057] A1. Treat the surface of the glass flakes with anionic surfactant, then wash and dry to obtain pretreated glass flakes.

[0058] A2. Add 30g of mixed powder of NaF, KF and NH4F to 100ml of 40% HF aqueous solution, stir until completely dissolved, and obtain an acid etching solution, wherein the mass ratio of NaF, KF and NH4F is 9:5:1.

[0059] A3. Place the pretreated glass flakes obtained in A1 into the acid etching solution obtained in A2, move the container into a super thermostat, immerse in a water bath at 25°C for 20 seconds, take out, rinse with hot water, and dry to obtain acid-etched glass flakes.

[0060] A4. Prepare the surface treatment agent into a 1% aqueous solution by mass, and add the acid-etched glass flakes obtained in A3 into it, soaking them completely for 5 minutes, take them out and dry them, and the modified glass flakes are obtained.

[0061] (2) Then, a long-lasting anticorrosive water-based coating is prepared, and the steps are as follows:

[0062] S1. Put 50 parts of water-based acrylic resin and 11 parts of water-based EVA emulsion into a dispersion tank by weight, control the temperature of the dispersion tank to 18° C., turn on the agitator, stir at a speed of 260 r / min, and stir for 30 min to uniformly mix the water-based acrylic resin and the water-based EVA emulsion to obtain a mixture a.

[0063] S2. According to the same standard of parts by weight, add 13 parts of modified glass flakes to the mixture a obtained in S1 under stirring, control the temperature of the dispersion tank to 24°C, adjust the stirring speed to 450r / min, and stir for 18min, then adjust the stirring speed to 560r / min, and stir for 24min to obtain a mixture b.

[0064] S3. According to the same standard weight proportions, add 1 part of leveling agent, 1 part of defoaming agent, 35 parts of water, 0.5 parts of thickener and 10 parts of anti-rust pigment to the mixture b obtained in S2 under stirring, control the temperature of the dispersion tank to 36°C, adjust the stirring speed to 340r / min, stir for 40min, and cool to obtain a long-lasting anticorrosive water-based coating.

[0065] Example 4: The difference between this example and Example 1 is that: (1) First, the modified glass flakes are prepared in the following steps:

[0066] A1. Treat the surface of the glass flakes with anionic surfactant, then wash and dry to obtain pretreated glass flakes.

[0067] A2. Add 30g of mixed powder of NaF, KF and NH4F to 100ml of 40% HF aqueous solution, stir until completely dissolved, and obtain an acid etching solution, wherein the mass ratio of NaF, KF and NH4F is 7:5:1.

[0068] A3. Place the pretreated glass flakes obtained in A1 into the acid etching solution obtained in A2, move the container into a super thermostat, immerse in a water bath at 25°C for 19 seconds, take out, rinse with hot water, and dry to obtain acid-etched glass flakes.

[0069] A4. Prepare the surface treatment agent into a 1% aqueous solution by mass, and add the acid-etched glass flakes obtained in A3 into it, soaking them completely for 5 minutes, take them out and dry them, and the modified glass flakes are obtained.

[0070] (2) Then, a long-lasting anticorrosive water-based coating is prepared, and the steps are as follows:

[0071] S1. Put 50 parts of water-based acrylic resin and 7 parts of water-based EVA emulsion into a dispersion tank by weight, control the temperature of the dispersion tank to 17° C., turn on the agitator, stir at a speed of 250 r / min, and stir for 25 min to uniformly mix the water-based acrylic resin and the water-based EVA emulsion to obtain a mixture a.

[0072] S2. According to the same standard of parts by weight, add 10 parts of modified glass flakes to the mixture a obtained in S1 under stirring, control the temperature of the dispersion tank to 23°C, adjust the stirring speed to 420r / min, and stir for 17min, then adjust the stirring speed to 470r / min, and stir for 22min to obtain a mixture b.

[0073] S3. According to the same standard weight parts, add 0.6 parts of leveling agent, 0.6 parts of defoaming agent, 32 parts of water, 0.4 parts of thickener and 8 parts of anti-rust pigment to the mixture b obtained in S2 under stirring, control the temperature of the dispersion tank to 33°C, adjust the stirring speed to 300r / min, stir for 35min, cool, and obtain a long-lasting anticorrosive water-based coating.

[0074] Example 5: The difference between this example and Example 1 is that: (1) First, the modified glass flakes are prepared in the following steps:

[0075] A1. Treat the surface of the glass flakes with anionic surfactant, then wash and dry to obtain pretreated glass flakes.

[0076] A2. Add 30g of mixed powder of NaF, KF and NH4F to 100ml of 40% HF aqueous solution, stir until completely dissolved, and obtain an acid etching solution, wherein the mass ratio of NaF, KF and NH4F is 9:3:1.

[0077] A3. Place the pretreated glass flakes obtained in A1 into the acid etching solution obtained in A2, move the container into a super thermostat, immerse in a water bath at 25°C for 12 seconds, take out, rinse with hot water, and dry to obtain acid-etched glass flakes.

[0078] A4. Prepare the surface treatment agent into a 1% aqueous solution by mass, and add the acid-etched glass flakes obtained in A3 into it, soaking them completely for 5 minutes, take them out and dry them, and the modified glass flakes are obtained.

[0079] (2) Then, a long-lasting anticorrosive water-based coating is prepared, and the steps are as follows:

[0080] S1. Put 40 parts of water-based acrylic resin and 11 parts of water-based EVA emulsion into a dispersion tank by weight, control the temperature of the dispersion tank to 18° C., turn on the agitator, stir at a speed of 260 r / min, and stir for 30 min to uniformly mix the water-based acrylic resin and the water-based EVA emulsion to obtain a mixture a.

[0081] S2. According to the same standard of parts by weight, add 8 parts of modified glass flakes to the mixture a obtained in S1 under stirring, control the temperature of the dispersion tank to 24°C, adjust the stirring speed to 450r / min, and stir for 12min, then adjust the stirring speed to 560r / min, and stir for 16min to obtain a mixture b.

[0082] S3. According to the same standard weight parts, add 0.8 parts of leveling agent, 0.8 parts of defoaming agent, 34 parts of water, 0.4 parts of thickener and 9 parts of anti-rust pigment to the mixture b obtained in S2 under stirring, control the temperature of the dispersion tank to 35°C, adjust the stirring speed to 320r / min, stir for 38min, cool, and obtain a long-lasting anticorrosive water-based coating.

[0083] Comparative Example 1: The difference between this comparative example and Example 1 is that the modified glass flakes are replaced by glass flakes.

[0084] Specifically, the steps for preparing the long-lasting anticorrosive water-based coating are as follows:

[0085] S1. Put 45 parts of water-based acrylic resin and 8 parts of water-based EVA emulsion into a dispersion tank by weight, control the temperature of the dispersion tank to 16° C., turn on the agitator, stir at a speed of 240 r / min, and stir for 22 min to uniformly mix the water-based acrylic resin and the water-based EVA emulsion to obtain a mixture a.

[0086] S2. According to the same standard of parts by weight, add 10 parts of glass flakes to the mixture a obtained in S1 under stirring, control the temperature of the dispersion tank to 22°C, adjust the stirring speed to 390r / min, stirring time for 15min, then adjust the stirring speed to 490r / min, stirring time for 20min, to obtain a mixture b.

[0087] S3. According to the same standard weight parts, add 0.7 parts of leveling agent, 0.5 parts of defoaming agent, 28 parts of water, 0.3 parts of thickener and 7 parts of anti-rust pigment to the mixture b obtained in S2 under stirring, control the temperature of the dispersion tank to 30°C, adjust the stirring speed to 300r / min, stir for 35min, cool, and obtain a long-lasting anticorrosive water-based coating.

[0088] Comparative Example 2: The difference between this comparative example and Example 1 is that the modified glass flakes are deleted.

[0089] Specifically, the steps for preparing the long-lasting anticorrosive water-based coating are as follows:

[0090] S1. Put 45 parts of water-based acrylic resin and 8 parts of water-based EVA emulsion into a dispersion tank by weight, control the temperature of the dispersion tank to 16° C., turn on the agitator, stir at a speed of 240 r / min, and stir for 22 min to uniformly mix the water-based acrylic resin and the water-based EVA emulsion to obtain a mixture a.

[0091] S2. According to the same standard weight parts, add 0.7 parts of leveling agent, 0.5 parts of defoaming agent, 28 parts of water, 0.3 parts of thickener and 7 parts of anti-rust pigment to the mixture a obtained in S1 under stirring, control the temperature of the dispersion tank to 30°C, adjust the stirring speed to 300r / min, stir for 35min, cool, and obtain a long-lasting anticorrosive water-based coating.

[0092] Comparative Example 3: The difference between this comparative example and Example 1 is that the aqueous EVA emulsion is deleted.

[0093] Specifically, the steps for preparing the long-lasting anticorrosive water-based coating are as follows:

[0094] S1. Add 10 parts of modified glass flakes to 45 parts of water-based acrylic resin by weight, control the temperature of the dispersion tank to 22°C, adjust the stirring speed to 390 r / min, stir for 15 min, then adjust the stirring speed to 490 r / min, stir for 20 min, and obtain a mixture b.

[0095] S2. According to the same standard weight parts, add 0.7 parts of leveling agent, 0.5 parts of defoaming agent, 28 parts of water, 0.3 parts of thickener and 7 parts of anti-rust pigment to the mixture b obtained in S1 under stirring, control the temperature of the dispersion tank to 30°C, adjust the stirring speed to 300r / min, stir for 35min, cool, and obtain a long-lasting anticorrosive water-based coating.

[0096] Comparative Example 4: This comparative example differs from Example 1 in that the modified glass flakes and the aqueous EVA emulsion are deleted.

[0097] Specifically, the steps for preparing the long-lasting anticorrosive water-based coating are as follows:

[0098] To 45 parts of water-based acrylic resin, add 0.7 parts of leveling agent, 0.5 parts of defoaming agent, 28 parts of water, 0.3 parts of thickener and 7 parts of anti-rust pigment by weight. Control the temperature of the dispersion tank to 30°C, adjust the stirring speed to 300r / min, stir for 35 minutes, and cool to obtain a long-lasting anticorrosive water-based coating.

[0099] Test example: Test items: 1. Anticorrosion performance;

[0100] 2. Low temperature resistance.

[0101] Test basis: GB / T 1771-2007.

[0102] Test method: 1. Anti-corrosion performance - expose the painted test panel to neutral salt spray to test the salt spray resistance; the larger the salt spray resistance test value, the better the anti-corrosion performance;

[0103] 2. Low temperature resistance - Two test panels coated with the same paint are recorded as X1 test panel and X2 test panel respectively; X1 test panel is directly exposed to neutral salt spray to test salt spray resistance data; X2 test panel is placed in a -20℃ environment for 24h and then exposed to neutral salt spray to test salt spray resistance data; calculate the low temperature loss rate of the salt spray resistance data of the two test panels, low temperature loss rate = (X1 data - X2 data) / X1 data * 100%; the smaller the low temperature loss rate value, the better the low temperature resistance performance.

[0104] Test results: See Table 1.

[0105] Table 1. Test data of the experimental example

[0106]

[0107]

[0108] Result analysis: Analyze examples 1-5 and combine the data in Table 1 and Figure 1-2 It can be seen that the water-based coating prepared by the present invention has both excellent anti-corrosion performance and low-temperature resistance; the salt spray resistance is as high as more than 856 hours, and the low-temperature loss rate is as low as less than 4.2%.

[0109] Analyze Example 1 and Comparative Examples 1-4 and combine the data in Table 1 and Figure 1 It can be seen that in the preparation of the water-based paint of the present invention, the addition of glass flakes can improve the anti-corrosion performance of the water-based paint; adding modified glass flakes obtained by the modification treatment of the glass flakes according to the present invention can further improve the anti-corrosion performance of the water-based paint; the addition of water-based EVA emulsion can also improve the anti-corrosion performance of the water-based paint; and the joint addition of modified glass flakes and water-based EVA emulsion can produce a synergistic effect and synergistically improve the anti-corrosion performance of the water-based paint.

[0110] Analyze Example 1 and Comparative Examples 1-4 and combine the data in Table 1 and Figure 2 It can be seen that the addition of water-based EVA emulsion can improve the low-temperature resistance of the water-based coating; adding glass flakes on the basis of the addition of water-based EVA emulsion can improve the low-temperature resistance of the water-based coating; on the basis of the addition of water-based EVA emulsion, the glass flakes are modified according to the present invention to obtain modified glass flakes, and then added to further improve the low-temperature resistance of the water-based coating; if the water-based EVA emulsion is not added, the addition of modified glass flakes will cause the low-temperature resistance of the water-based coating to decrease instead of increase.

[0111] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0112] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A long-lasting anti-corrosion water-based coating, It is characterized in that The raw material components are as follows, measured by weight: 40-50 parts of water-based acrylic resin, 7-11 parts of water-based EVA emulsion, 8-13 parts of modified glass flakes, 0.1-1 parts of leveling agent, 0.1-1 parts of defoaming agent, 20-35 parts of water, 0.1-0.5 parts of thickener and 5-10 parts of anti-rust pigment.

2. The long-lasting anticorrosive water-based coating according to claim 1, It is characterized in that The preparation method of the modified glass flakes is as follows: A1. Treat the surface of the glass flakes with an anionic surfactant, then rinse with deionized water and dry to obtain pretreated glass flakes; A2. Add 30 g of NaF, KF and NH to 100 ml of 40% HF aqueous solution. 4 Mix the powders F and stir until they are completely dissolved to obtain an acid etching solution; A3, put the pretreated glass flakes obtained in A1 into the acid etching solution obtained in A2, move the container into a super thermostat, immerse in a water bath at 25°C for 10-20s, take out, rinse with hot water, and dry to obtain acid-etched glass flakes; A4. Prepare the surface treatment agent into a 1% aqueous solution by mass, and add the acid-etched glass flakes obtained in A3 into it, soaking them completely for 5 minutes, take them out and dry them, and the modified glass flakes are obtained.

3. The long-lasting anticorrosive water-based coating according to claim 2, It is characterized in that In A1, the anionic surfactant is sodium dodecylbenzene sulfonate.

4. The long-lasting anticorrosive water-based coating according to claim 2, It is characterized in that In A2, NaF, KF and NH 4 The mass ratio of F is (7-9):(3-5):

1.

5. The long-lasting anticorrosive water-based coating according to claim 2, It is characterized in that In A4, the surface treatment agent is silane coupling agent KH-550.

6. The long-lasting anticorrosive water-based coating according to claim 1, It is characterized in that The leveling agent is an aromatic alkylsiloxane leveling agent.

7. The long-lasting anticorrosive water-based coating according to claim 1, It is characterized in that The defoamer is an organosilicon defoamer.

8. The long-lasting anticorrosive water-based coating according to claim 1, It is characterized in that The thickener is carboxymethyl cellulose.

9. The long-lasting anticorrosive water-based coating according to claim 1, It is characterized in that The anti-rust pigment is any one of mica iron oxide, zinc phosphate and aluminum tripolyphosphate.

10. A method for preparing the long-lasting anticorrosive water-based coating according to any one of claims 1 to 9, It is characterized in that The following steps are involved: S1. Add water-based acrylic resin and water-based EVA emulsion into a dispersion tank, control the temperature of the dispersion tank to 15-18° C., start the agitator, stir at a speed of 220-260 r / min, stir for 18-30 min, and obtain a mixture a; S2, add modified glass flakes to the mixture a obtained in S1, control the temperature of the dispersion tank to 20-24°C, adjust the stirring speed to 350-450r / min, stir for 12-18min, then adjust the stirring speed to 460-560r / min, stir for 16-24min, and obtain a mixture b; S3. Add leveling agent, defoaming agent, water, thickener and anti-rust pigment to the mixture b obtained in S2, control the temperature of the dispersion tank to 26-36°C, adjust the stirring speed to 280-340r / min, stir for 30-40min, and cool to obtain a long-lasting anticorrosive water-based coating.

Citation Information

Patent Citations

  • Waterborne coating for wood and preparation method thereof

    CN106675260A

  • High-temperature-resistant fireproof basalt flake coating and preparation method thereof

    CN114773950A

  • Corrosion-resistant raw lacquer coating as well as preparation method and application thereof

    CN115851129A

  • Coating Composition for Absorbing Infrared Rays

    KR1020170041294A

  • Rust inhibitor with excellent adhesion performance

    KR102065604B1